{"id":20871,"date":"2026-10-04T07:21:27","date_gmt":"2026-10-03T23:21:27","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20871"},"modified":"2026-10-10T23:39:07","modified_gmt":"2026-10-10T15:39:07","slug":"tool-steel-heat-treating-practices","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treating-practices\/","title":{"rendered":"\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uc2e4\ubb34"},"content":{"rendered":"\n<style> :root{ --aobo-accent:#2563eb; --aobo-accent-dark:#1e1e2e; --aobo-blue:#0c56d0; --aobo-blue-dark:#073b91; --aobo-text:#333; --aobo-muted:#888; --aobo-border:#e5e7eb; --aobo-border-dark:#ddd; --aobo-stripe:#f7f7f9; --aobo-hover:#e8f0fe; --aobo-radius:8px; --aobo-radius-sm:6px; --aobo-orange:#f59e0b; --aobo-fill:#e9ecef; } *{box-sizing:border-box;} html{-webkit-text-size-adjust:100%;} body{margin:0;background:#fff;color:var(--aobo-text); font-family:-apple-system,BlinkMacSystemFont,\"Segoe UI\",Roboto,\"Helvetica Neue\",Arial,sans-serif; font-size:15px;line-height:1.6;} \/* Root scope \u2014 WordPress theme guard *\/ .ts-props{color:var(--aobo-text);background:transparent;padding:0;box-sizing:border-box;line-height:1.6;} .ts-props *{box-sizing:border-box;} .ts-props button,.ts-props input[type=\"text\"]{ background:none !important;border:none !important;border-radius:0 !important;padding:0 !important; margin:0 !important;font-size:inherit !important;font-weight:inherit !important; letter-spacing:normal !important;text-transform:none !important;box-shadow:none !important; line-height:inherit !important;text-decoration:none !important;} .aobo-wrap{max-width:1160px;margin:0 auto;} \/* Hero *\/ .ts-hero{background:#fff;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);overflow:hidden;} .ts-hero-top{padding:1.5em;background:var(--aobo-stripe);border-bottom:1px solid var(--aobo-border);} .ts-kicker{display:inline-flex;align-items:center;gap:6px;color:var(--aobo-accent);background:var(--aobo-hover); border:1px solid var(--aobo-border);border-radius:var(--aobo-radius-sm);padding:4px 8px; font-size:.85em;font-weight:600;margin-bottom:.8em;} .ts-kicker span{width:6px;height:6px;background:var(--aobo-orange);border-radius:50%;display:inline-block;} .ts-hero h1{margin:0;font-size:2rem;line-height:1.3;color:var(--aobo-text);text-align:center;} .ts-hero-top p{margin:.6em auto 0;max-width:820px;font-size:.9em;line-height:1.6;color:var(--aobo-muted);text-align:center;} \/* Tool area *\/ .ts-tool-area{padding:1.5em;} \/* Legend *\/ .ts-legend{display:flex;flex-wrap:wrap;gap:8px;margin-bottom:1em;} .ts-legend > span{display:inline-flex;align-items:center;gap:5px;font-size:.8em;color:var(--aobo-muted); background:var(--aobo-stripe);border:1px solid var(--aobo-border);border-radius:var(--aobo-radius-sm); padding:3px 8px;} .ts-legend b{color:var(--aobo-text);font-weight:600;} .ts-legend .ts-dot{width:9px;height:9px;border-radius:50%;background:var(--aobo-accent);display:inline-block; padding:0;border:0;gap:0;} \/* Controls *\/ .ts-controls{display:flex;flex-wrap:wrap;gap:10px;align-items:center;background:var(--aobo-stripe); border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);padding:1em;margin-bottom:1.2em;} .ts-search{flex:1 1 220px;max-width:340px;position:relative;} .ts-props .ts-search input{width:100% !important;border:1px solid var(--aobo-border-dark) !important; border-radius:var(--aobo-radius-sm) !important;padding:.5em .6em .5em 2em !important; font-size:.92em !important;color:var(--aobo-text) !important;background:#fff !important; outline:none !important;box-shadow:none !important;} .ts-props .ts-search input:focus{border-color:var(--aobo-accent) !important; box-shadow:0 0 0 2px rgba(37,99,235,.12) !important;} .ts-search::before{content:\"\";position:absolute;left:.7em;top:50%;transform:translateY(-50%); width:13px;height:13px;background:var(--aobo-muted); -webkit-mask:url(\"data:image\/svg+xml;utf8,<svg xmlns='http:\/\/www.w3.org\/2000\/svg' viewBox='0 0 24 24' fill='none' stroke='black' stroke-width='2'><circle cx='11' cy='11' r='8'\/><path d='m21 21-4.3-4.3'\/><\/svg>\") center\/contain no-repeat; mask:url(\"data:image\/svg+xml;utf8,<svg xmlns='http:\/\/www.w3.org\/2000\/svg' viewBox='0 0 24 24' fill='none' stroke='black' stroke-width='2'><circle cx='11' cy='11' r='8'\/><path d='m21 21-4.3-4.3'\/><\/svg>\") center\/contain no-repeat;} .ts-chips{display:flex;flex-wrap:wrap;gap:6px;} .ts-props .ts-chip{border:1px solid var(--aobo-border-dark) !important;background:#fff !important; color:var(--aobo-text) !important;border-radius:999px !important;padding:.4em .9em !important; font-size:.8em !important;font-weight:600 !important;cursor:pointer !important;transition:all .15s !important;} .ts-props .ts-chip:hover{background:var(--aobo-hover) !important;border-color:var(--aobo-accent) !important;} .ts-props .ts-chip.on{background:var(--aobo-accent) !important;border-color:var(--aobo-accent) !important;color:#fff !important;} .ts-count{font-size:.8em;color:var(--aobo-muted);margin-left:auto;white-space:nowrap;} \/* Table *\/ .ts-table-wrap{overflow-x:auto;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius); background:#fff;box-shadow:0 1px 2px rgba(16,24,40,.04);} table.ts-table{border-collapse:collapse;width:100%;min-width:880px;font-size:.88em;} .ts-table thead th{position:sticky;top:0;z-index:2;background:var(--aobo-accent-dark);color:#fff; border-bottom:0;border-right:1px solid rgba(255,255,255,.1);text-align:center;padding:.6em .7em; font-size:.82em;font-weight:600;text-transform:none;letter-spacing:.02em;cursor:pointer; white-space:nowrap;user-select:none;} .ts-table thead th:last-child{border-right:0;} .ts-table thead th .ts-arr{color:#ffd166;font-weight:700;margin-left:3px;} .ts-table tbody td{padding:.55em .7em;border-bottom:1px solid var(--aobo-border);text-align:center; vertical-align:middle;white-space:nowrap;} .ts-table tbody tr:nth-child(even){background:var(--aobo-stripe);} .ts-table tbody tr:hover{background:var(--aobo-hover);} .ts-table tbody tr.ts-group td{background:#e8ecf1;font-weight:700;font-size:.78em;letter-spacing:.05em; text-transform:uppercase;color:#3c4043;padding:.55em .7em;border-bottom:1px solid var(--aobo-border); text-align:left;} .ts-table tbody tr:not(.ts-group).ts-hide{display:none;} td.ts-grade{font-weight:700;font-size:.95em;text-align:left;white-space:nowrap;color:var(--aobo-text);} .ts-meter{display:inline-flex;align-items:center;gap:7px;} .ts-meter i{display:inline-block;width:44px;height:6px;border-radius:3px;background:var(--aobo-fill);overflow:hidden;} .ts-meter i b{display:block;height:100%;border-radius:3px;background:linear-gradient(90deg,#4d94ff,var(--aobo-accent));} .ts-meter span{font-size:.9em;font-weight:600;min-width:14px;} .ts-hr{font-variant-numeric:tabular-nums;font-weight:500;} .ts-num{font-variant-numeric:tabular-nums;} .ts-sup{font-size:9px;color:var(--aobo-accent);vertical-align:super;line-height:0;} \/* Footnotes *\/ .ts-notes-list{margin:1.2em 0 0;background:#fff;border:1px solid var(--aobo-border); border-left:3px solid var(--aobo-accent);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0; padding:1em 1.2em 1em 2.2em;font-size:.82em;color:var(--aobo-muted);line-height:1.7;} .ts-notes-list li{margin-bottom:.3em;} .ts-notes-list sup{color:var(--aobo-accent);font-size:10px;} \/* Figure *\/ .ts-fig{margin:1.2em 0 0;background:#fff;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);padding:1em;} .ts-fig img{display:block;width:100%;height:auto;border-radius:6px;} .ts-fig figcaption{font-size:.8em;color:var(--aobo-muted);margin-top:.6em;line-height:1.6;} .ts-fig figcaption b{color:var(--aobo-text);} \/* Info cards *\/ .ts-grid{display:grid;grid-template-columns:repeat(auto-fit,minmax(250px,1fr));gap:14px;margin-top:1.2em;} .ts-grid .ts-card{background:#fff;border:1px solid var(--aobo-border);border-left:3px solid var(--aobo-accent); border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;padding:1em 1.2em;} .ts-grid h2{font-size:1em;margin:0 0 .4em;color:var(--aobo-text);} .ts-grid p{font-size:.82em;color:var(--aobo-muted);margin:0;line-height:1.7;} .ts-grid p b{color:var(--aobo-text);font-weight:600;} \/* Disclaimer *\/ .ts-disclaimer{margin-top:1.2em;background:#fff;border:1px solid var(--aobo-border); border-left:3px solid var(--aobo-accent);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0; padding:1em 1.2em;} .ts-disclaimer h3{margin:0 0 .5em;font-size:.95em;color:var(--aobo-text);display:flex;align-items:center;gap:6px;} .ts-disclaimer h3::before{content:\"\\2139\";font-size:1em;color:var(--aobo-accent);} .ts-disclaimer p{margin:0 0 .5em;max-width:none;color:var(--aobo-muted);line-height:1.7;} .ts-disclaimer p:last-child{margin-bottom:0;} \/* Empty \/ source *\/ .ts-empty{display:none;text-align:center;color:var(--aobo-muted);padding:2em 1em;font-size:.9em;} .ts-empty.show{display:block;} .ts-source{margin-top:.8em;color:var(--aobo-muted);font-size:.82em;line-height:1.58;} @media (max-width:860px){ .ts-hero-top,.ts-tool-area{padding:1em;} .ts-controls{flex-direction:column;align-items:stretch;} .ts-search{max-width:none;} .ts-count{margin-left:0;} .ts-hero h1{font-size:1.5rem;} } @media (max-width:520px){ .ts-hero-top,.ts-tool-area{padding:.8em;} table.ts-table{font-size:.82em;} .ts-table thead th,.ts-table tbody td{padding:.4em .4em;} } table.ts-table thead th{cursor:default;} table.ts-table td.ts-grade{font-weight:700;} table.ts-table td.ts-type{white-space:normal;text-align:left;font-size:.92em;color:#555;min-width:150px;} table.ts-table td.ts-long{white-space:normal;text-align:left;vertical-align:top;font-size:.92em;color:#444; min-width:260px;line-height:1.55;} table.ts-table td.ts-safe{white-space:normal;text-align:left;vertical-align:top;} table.ts-table tbody tr:hover{background:var(--aobo-hover);} table.ts-table tbody tr.ts-group:hover td{background:#e8ecf1;} .ts-sec{margin:1.8em 0 .5em;font-size:1.02em;color:var(--aobo-text);font-weight:700;} .ts-sec span{display:block;font-size:.8em;font-weight:400;color:var(--aobo-muted);margin-top:.15em;line-height:1.6;} .ts-table-wrap{margin-top:.6em;} .ts-tcap{margin:.5em 0 0;font-size:.78em;color:var(--aobo-muted);line-height:1.6;} .ts-props a{color:var(--aobo-blue) !important;text-decoration:none !important;} .ts-props a:hover{text-decoration:underline !important;} .ts-rel{margin-top:1.2em;background:#fff;border:1px solid var(--aobo-border); border-left:3px solid var(--aobo-blue);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;padding:1em 1.2em;} .ts-rel h3{margin:0 0 .5em;font-size:.95em;color:var(--aobo-text);} .ts-rel p{margin:0;font-size:.85em;line-height:1.9;color:var(--aobo-muted);} .ts-rel p a{font-weight:600;} .aobo-ht-ref.ts-props table.ts-table.wraphead thead th{white-space:normal;line-height:1.25;} .aobo-ht-ref.ts-props table.ts-table.wraphead tbody td{white-space:nowrap !important;}\n<\/style> <style id=\"aobo-dl-css\">\n.aobo-ht-ref.ts-props .ts-dl{display:flex !important;flex-wrap:wrap;align-items:center;gap:1em; background:var(--aobo-stripe) !important;border:1px solid var(--aobo-border) !important; border-radius:var(--aobo-radius) !important;padding:1.1em 1.3em !important;margin:1.5em 0 !important;}\n.aobo-ht-ref.ts-props .ts-dl-txt{flex:1 1 340px;font-size:.95em;color:var(--aobo-text) !important;line-height:1.55;}\n.aobo-ht-ref.ts-props .ts-dl-txt strong{display:block;font-weight:700 !important;margin-bottom:.2em;color:var(--aobo-text) !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn{display:inline-flex !important;align-items:center;gap:.5em; background:var(--aobo-blue) !important;color:#fff !important;border:1px solid var(--aobo-blue) !important; border-radius:var(--aobo-radius-sm) !important;padding:.75em 1.35em !important;font-size:.95em !important; font-weight:600 !important;text-decoration:none !important;white-space:nowrap;box-shadow:none !important; line-height:1.3 !important;text-transform:none !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn:hover,.aobo-ht-ref.ts-props a.ts-dl-btn:focus{background:var(--aobo-blue-dark) !important; border-color:var(--aobo-blue-dark) !important;color:#fff !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn svg{width:1.05em;height:1.05em;fill:none;stroke:currentColor;stroke-width:2;flex:0 0 auto;}\n@media (max-width:640px){.aobo-ht-ref.ts-props a.ts-dl-btn{width:100%;justify-content:center;}}\n<\/style> <style id=\"aobo-ds\">\n.entry-content[class]{--ds-font-body: Lora,serif;--ds-font-head: Lato,sans-serif;--ds-blue: #0c56d0;--ds-blue-deep: #082d6f;--ds-blue-dark: #073b91;--ds-blue-soft: #eaf2ff;--ds-blue-pale: #f7fbff;--ds-border: #d7e5fb;--ds-border-soft: #e8eef8;--ds-text: #203044;--ds-muted: #617087;--ds-orange: #f59b23;--ds-shadow: 0 18px 45px rgba(12,86,208,0.10);--ds-shadow-sm: 0 12px 32px rgba(12,86,208,0.07);font-family: var(--ds-font-body);line-height: 1.7;-webkit-text-size-adjust: 100%;box-sizing: border-box}.entry-content[class] *,.entry-content[class] *::before,.entry-content[class] *::after{box-sizing: border-box}.entry-content[class] h1{font-family: var(--ds-font-head) !important;font-size: clamp(24px,4vw,min(50px,var(--h1-max,50px))) !important;line-height: 1.08 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 0 0 16px !important}.entry-content[class] h2{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 44px 0 16px !important}.entry-content[class] h3{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.3 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 30px 0 12px !important}.entry-content[class] h4{font-family: var(--ds-font-head) !important;font-size: 19px !important;line-height: 1.35 !important;letter-spacing: 0 !important;font-weight: 700 !important;margin: 24px 0 10px !important}.entry-content[class] p,.entry-content[class] li,.entry-content[class] dd,.entry-content[class] dt{font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important}.entry-content[class] figcaption,.entry-content[class] small,.entry-content[class] .aobo-figure figcaption{font-size: 15px !important;line-height: 1.6 !important}.entry-content[class] table{width: 100%;border-collapse: collapse;background: #ffffff}.entry-content[class] table th,.entry-content[class] table thead th,.entry-content[class] table thead td{background: var(--ds-blue-soft) !important;color: var(--ds-blue-deep) !important;font-family: var(--ds-font-head) !important;font-size: 15px !important;font-weight: 700 !important;line-height: 1.45 !important;text-align: center !important;text-transform: none !important;letter-spacing: 0 !important;padding: 14px 16px !important;border: 0 !important;border-bottom: 1px solid var(--ds-border) !important;vertical-align: top !important;position: static !important}.entry-content[class] table td{font-family: var(--ds-font-body) !important;font-size: 15px !important;line-height: 1.55 !important;padding: 14px 16px !important;border: 0;border-bottom: 1px solid var(--ds-border-soft) !important;vertical-align: top !important;white-space: normal !important;text-align: center !important}.entry-content[class] table tbody tr:last-child td{border-bottom: 0 !important}.entry-content[class] table th.ds-text,.entry-content[class] table td.ds-text{text-align: left !important}.entry-content[class] table tbody tr:nth-child(even){background: #fafcff !important}.entry-content[class] table tbody tr:hover{background: #f2f7ff !important}.entry-content[class] table tbody td:first-child{color: var(--ds-blue-deep);font-weight: 700}.entry-content[class] .aobo-table-wrap,.entry-content[class] .ts-table-wrap{overflow-x: auto;margin: 22px 0 28px;border: 1px solid var(--ds-border);border-radius: 18px;box-shadow: var(--ds-shadow-sm);background: #ffffff}.entry-content[class] h1,.entry-content[class] h2,.entry-content[class] h3,.entry-content[class] h4{color: var(--ds-blue-deep)}.entry-content[class] p,.entry-content[class] li{color: var(--ds-text)}.entry-content[class] a{color: var(--ds-blue);font-weight: 700;text-decoration: none}.entry-content[class] a:hover,.entry-content[class] a:focus{color: var(--ds-orange)}.entry-content[class] .aobo-final-cta h1,.entry-content[class] .aobo-final-cta h2,.entry-content[class] .aobo-final-cta h3,.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-cta h1,.entry-content[class] .aobo-cta h2,.entry-content[class] .aobo-cta h3,.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-cta-buttons,.entry-content[class] .aobo-cta-buttons *,.entry-content[class] .aobo-esr .stat-band h2,.entry-content[class] .aobo-esr .stat-band h3,.entry-content[class] .aobo-esr .stat-band p,.entry-content[class] .aobo-esr .closing h2,.entry-content[class] .aobo-esr .closing h3,.entry-content[class] .aobo-esr .closing p,.entry-content[class] .footcta h2,.entry-content[class] .footcta h3,.entry-content[class] .footcta p,.entry-content[class] .bg-dark h2,.entry-content[class] .bg-dark h3,.entry-content[class] .bg-dark p,.entry-content[class] .ht-header h2,.entry-content[class] .ht-header h3,.entry-content[class] .ts-cta h2,.entry-content[class] .ts-cta h3,.entry-content[class] .aobo-sup .stats h2,.entry-content[class] .aobo-sup .stats h3,.entry-content[class] .aobo-sup .stats p,.entry-content[class] .aobo-sup .cta h2,.entry-content[class] .aobo-sup .cta h3,.entry-content[class] .aobo-sup .cta p{color: inherit}.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-sup .cta p{color: rgba(255,255,255,0.92)}.entry-content[class] .has-ast-global-color-0-background-color,.entry-content[class] .has-ast-global-color-0-background-color *,.entry-content[class] .contact-container,.entry-content[class] .contact-container *{color: #ffffff !important}.entry-content[class] .has-ast-global-color-0-background-color .label-text,.entry-content[class] .has-ast-global-color-0-background-color .label-text *,.entry-content[class] .contact-container .label-text{color: rgba(255,255,255,0.72) !important}.entry-content[class] .aobo-cta h1,.entry-content[class] .aobo-cta h2,.entry-content[class] .aobo-cta h3,.entry-content[class] .aobo-cta h4,.entry-content[class] .cta h1,.entry-content[class] .cta h2,.entry-content[class] .cta h3,.entry-content[class] .cta h4,.entry-content[class] .aobo-final-cta h1,.entry-content[class] .aobo-final-cta h2,.entry-content[class] .aobo-final-cta h3,.entry-content[class] .aobo-final-cta h4{color: #ffffff !important}.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-cta li,.entry-content[class] .cta p,.entry-content[class] .cta li,.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-final-cta li{color: rgba(255,255,255,0.93) !important}.entry-content[class] .aobo-cta p a,.entry-content[class] .aobo-cta li a,.entry-content[class] .cta p a,.entry-content[class] .cta li a,.entry-content[class] .aobo-final-cta p a,.entry-content[class] .aobo-final-cta li a{color: #ffffff !important;text-decoration: underline}.entry-content[class] .aobo-btn-inquiry{color: #ffffff !important}.entry-content[class] .aobo-cta .aobo-btn-inquiry,.entry-content[class] .aobo-final-cta .aobo-btn-inquiry{color: var(--ds-blue) !important}.entry-content[class] .aobo-wrap,.entry-content[class] .aobo-article{max-width: 1180px;margin: 0 auto;padding: 0}.entry-content[class] img{max-width: 100%;height: auto}.entry-content[class] figure{margin: 26px auto 34px;max-width: 860px}.entry-content[class] figure img{display: block;width: 100%;border: 1px solid var(--ds-border);border-radius: 18px;box-shadow: var(--ds-shadow-sm);background: #ffffff}.entry-content[class] .aobo-hero{background: linear-gradient(135deg,#ffffff 0%,#f7fbff 56%,#eaf2ff 100%);border: 1px solid var(--ds-border);border-radius: 28px;padding: 42px 38px;margin-bottom: 24px;box-shadow: var(--ds-shadow);overflow: hidden;position: relative}.entry-content[class] .aobo-hero::after{content: \"\";position: absolute;right: -90px;top: -90px;width: 260px;height: 260px;border-radius: 50%;background: rgba(12,86,208,0.08)}.entry-content[class] .aobo-hero h1,.entry-content[class] .aobo-hero p{position: relative;z-index: 2}.entry-content[class] .aobo-note-box{margin: 34px 0;padding: 22px 24px;border: 1px solid var(--ds-border);border-left: 5px solid var(--ds-orange);border-radius: 16px;background: #fbfdff}.entry-content[class] .aobo-note-box p{margin: 0 0 14px;color: var(--ds-muted) !important;font-style: italic}.entry-content[class] .aobo-note-box p:last-child{margin-bottom: 0}.entry-content[class] .aobo-btn{display: inline-flex;align-items: center;justify-content: center;min-height: 42px;padding: 10px 16px;border-radius: 999px;text-align: center;text-decoration: none;font-family: var(--ds-font-head) !important;font-weight: 700;font-size: 14px !important;line-height: 1.2;transition: all 0.2s ease;cursor: pointer;white-space: nowrap}.entry-content[class] .aobo-btn-primary{background: var(--ds-blue);border: 1px solid var(--ds-blue);color: #ffffff !important}.entry-content[class] .aobo-btn-secondary{background: #ffffff;border: 1px solid var(--ds-border);color: var(--ds-blue) !important}.entry-content[class] .aobo-btn:hover{transform: translateY(-1px)}.entry-content[class] .aobo-supply-actions{display: flex;flex-wrap: wrap;gap: 12px;margin-top: 18px}.entry-content[class] .aobo-supply-actions .aobo-btn{min-width: 190px}.entry-content[class] .aobo-final-cta{margin-top: 34px;padding: 34px;border-radius: 28px;background: linear-gradient(135deg,#073b91 0%,#0c56d0 100%);box-shadow: 0 18px 45px rgba(12,86,208,0.20);display: flex;align-items: center;justify-content: space-between;gap: 20px;flex-wrap: wrap}.entry-content[class] .aobo-final-cta h2{margin: 0 0 12px !important;font-size: 26px !important;color: #ffffff !important}.entry-content[class] .aobo-final-cta p{margin: 0}.entry-content[class] .aobo-final-cta .aobo-btn-primary{background: #ffffff;border-color: #ffffff;color: var(--ds-blue) !important}.entry-content[class] .aobo-final-cta .aobo-btn-secondary{background: transparent;border-color: rgba(255,255,255,0.75);color: #ffffff !important}.entry-content[class] .ts-hero{background: transparent !important;border: 0 !important;border-radius: 0 !important;box-shadow: none !important}.entry-content[class] .ts-hero-top{background: linear-gradient(135deg,#ffffff 0%,#f7fbff 56%,#eaf2ff 100%) !important;border: 1px solid var(--ds-border) !important;border-radius: 28px !important;padding: 42px 38px !important;margin: 0 0 24px !important;box-shadow: var(--ds-shadow) !important;position: relative;overflow: hidden;text-align: left !important}.entry-content[class] .ts-hero-top h1,.entry-content[class] .ts-hero-top p,.entry-content[class] .ts-hero h1{text-align: left !important}.entry-content[class] .ts-hero-top p{max-width: none !important;margin: 0 0 12px !important}.entry-content[class] .ts-tool-area{padding: 0 !important}.entry-content[class] .ts-sec{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 44px 0 16px !important}.entry-content[class] .ts-sec > span{display: block !important;font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important;font-weight: 400 !important;color: var(--ds-text) !important;margin: 0 0 16px !important}.entry-content[class] .ts-kicker{display: inline-flex !important;align-items: center;gap: 7px;margin: 0 0 14px !important;padding: 6px 14px !important;border: 1px solid var(--ds-border) !important;border-radius: 999px !important;background: #ffffff !important;color: var(--ds-blue) !important;font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important;letter-spacing: 0 !important;text-transform: none !important}.entry-content[class] .ts-p,.entry-content[class] .card-desc,.entry-content[class] .aobo-strip-intro,.entry-content[class] .schema-faq-answer{font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important;font-weight: 400 !important}.entry-content[class] .lead,.entry-content[class] .fund-lead{font-family: var(--ds-font-body) !important;font-size: 19px !important;line-height: 1.65 !important;font-weight: 400 !important}.entry-content[class] .ts-h2{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 44px 0 16px !important}.entry-content[class] .ts-h3{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.3 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 30px 0 12px !important}.entry-content[class] .card-grade{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.25 !important;font-weight: 700 !important}.entry-content[class] .schema-faq-question{font-family: var(--ds-font-head) !important;font-size: 19px !important;line-height: 1.4 !important;font-weight: 700 !important;color: var(--ds-blue-deep) !important}.entry-content[class] .ts-source,.entry-content[class] .ts-hint,.entry-content[class] .ts-placeholder,.entry-content[class] .ht-spec-label,.entry-content[class] .ht-spec-value,.entry-content[class] .ht-step-indicator,.entry-content[class] .ht-badge,.entry-content[class] .idx,.entry-content[class] .xlink,.entry-content[class] .cat-note,.entry-content[class] .aobo-card-note,.entry-content[class] .card-desig,.entry-content[class] .k,.entry-content[class] .v,.entry-content[class] .note,.entry-content[class] .aobo-note{font-family: var(--ds-font-head) !important;font-size: 15px !important;line-height: 1.6 !important;font-weight: 400 !important}.entry-content[class] .ht-spec-label,.entry-content[class] .idx,.entry-content[class] .k{font-weight: 700 !important}.entry-content[class] .aobo-note,.entry-content[class] .note{font-family: var(--ds-font-body) !important;color: var(--ds-muted) !important}.entry-content[class] .chip{font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important}.entry-content[class] .kicker,.entry-content[class] .eyebrow,.entry-content[class] .aobo-eyebrow{display: inline-flex !important;align-items: center;gap: 7px;margin: 0 0 14px !important;padding: 6px 14px !important;border: 1px solid var(--ds-border) !important;border-radius: 999px !important;background: #ffffff !important;color: var(--ds-blue) !important;font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important;letter-spacing: 0 !important;text-transform: none !important}@media (max-width: 760px){.entry-content[class] h1{font-size: clamp(22px,6.4vw,min(34px,var(--h1-max,34px))) !important}.entry-content[class] h2{font-size: 25px !important}.entry-content[class] h3{font-size: 20px !important}.entry-content[class] h4{font-size: 17px !important}.entry-content[class] p,.entry-content[class] li{font-size: 16px !important}.entry-content[class] table th,.entry-content[class] table td{font-size: 14px !important;padding: 11px 12px !important}.entry-content[class] .aobo-hero{padding: 30px 22px}.entry-content[class] .aobo-final-cta{padding: 26px 22px}.entry-content[class] .aobo-final-cta .aobo-btn{width: 100%}}\n<\/style>\n<section class=\"aobo-ht-ref ts-props\">\n<div class=\"aobo-wrap\"> <div class=\"ts-hero\">\n<div class=\"ts-hero-top\">\n<div class=\"ts-kicker\"><span><\/span>Tool Steel | Heat Treating Practice<\/div>\n<h1 style=\"--h1-max:44px\">Tool Steel Heat Treating Practices<\/h1>\n<p>A tool steel performs the way its heat treating cycle prepared it, and most of the tool life that is lost in a shop is lost in the hours between the quench and the final temper. The tables on this page are the published practice data for that part of the route. They cover the safe delay between quenching and tempering, <a href=\"https:\/\/aobosteel.com\/cycle-annealing-tool-steel\/\">isothermal cycle annealing schedules<\/a>, the time a load needs to reach the tempering temperature, <a href=\"https:\/\/aobosteel.com\/automated-heat-treating-tool-steel\/\">the cycle times of an automated salt bath line for high speed steel<\/a>, the endothermic atmosphere dew point that protects the surface during hardening, and <a href=\"https:\/\/aobosteel.com\/packing-compounds-annealing-tool-steel\/\">the packing compounds used when a tool is annealed in a pack<\/a>. Every figure is reproduced from the source tables and the source article, table number is given under each one so the original can be checked.<\/p>\n<\/div>\n<\/div> <div class=\"ts-tool-area\"> <h2 class=\"ts-h2\">Time between quenching and tempering<\/h2>\n<p class=\"ts-p\">Shock resisting tool steels are the grades most exposed to cracking in the interval after the quench. The steel has just transformed to martensite and the section carries the full transformation stress, and a water or a brine quench adds thermal stress on top of it. Tempering is what relieves that stress, so the delay before the tempering furnace is a process limit that belongs on the route card. The figures in Table 1 were measured in one plant on the S grades, and they show how quickly the allowance falls as the austenitizing temperature and the severity of the quench go up. The same plant found that a double temper is worth the extra cycle on the S steels, with the first temper run 30 to 55 &deg;C (50 to 100 &deg;F) below the second.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:660px;\">\n<thead><tr><th>Steel<\/th><th>Austenitizing temperature, &deg;C<\/th><th>Austenitizing temperature, &deg;F<\/th><th>Quenching medium<\/th><th>Allowable time prior to tempering, min<\/th><\/tr><\/thead>\n<tbody>\n<tr><td class=\"ts-grade\">S1<\/td><td>900<\/td><td>1650<\/td><td>Oil<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-grade\">S1<\/td><td>980<\/td><td>1800<\/td><td>Oil<\/td><td class=\"ts-num\">15<\/td><\/tr>\n<tr><td class=\"ts-grade\">S2<\/td><td>845<\/td><td>1550<\/td><td>Brine<\/td><td class=\"ts-num\">10<\/td><\/tr>\n<tr><td class=\"ts-grade\">S2<\/td><td>900<\/td><td>1650<\/td><td>Brine<\/td><td class=\"ts-num\">5<\/td><\/tr>\n<tr><td class=\"ts-grade\">S3<\/td><td>815<\/td><td>1500<\/td><td>Brine<\/td><td class=\"ts-num\">10<\/td><\/tr>\n<tr><td class=\"ts-grade\">S3<\/td><td>870<\/td><td>1600<\/td><td>Brine<\/td><td class=\"ts-num\">5<\/td><\/tr>\n<tr><td class=\"ts-grade\">S4<\/td><td>870<\/td><td>1600<\/td><td>Brine<\/td><td class=\"ts-num\">10<\/td><\/tr>\n<tr><td class=\"ts-grade\">S4<\/td><td>925<\/td><td>1700<\/td><td>Brine<\/td><td class=\"ts-num\">5<\/td><\/tr>\n<tr><td class=\"ts-grade\">S4<\/td><td>900<\/td><td>1650<\/td><td>Oil<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-grade\">S4<\/td><td>955<\/td><td>1750<\/td><td>Oil<\/td><td class=\"ts-num\">15<\/td><\/tr>\n<tr><td class=\"ts-grade\">S5<\/td><td>870<\/td><td>1600<\/td><td>Oil<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-grade\">S5<\/td><td>925<\/td><td>1700<\/td><td>Oil<\/td><td class=\"ts-num\">15<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 3 of Heat Treating of Specific Classes of Tool Steels. Values determined by an extensive study conducted in one plant. The source notes that the allowable time may vary significantly with the size and shape of the part.<\/em><\/p> <h2 class=\"ts-h2\">Cycle annealing schedules<\/h2>\n<p class=\"ts-p\">Cycle annealing replaces a long slow furnace cool with two isothermal holds in the transformation range. It gives little advantage on a large load, because the centre of the load still has to come down slowly, but for a single tool that can be handled in a liquid bath or a small furnace it saves a substantial amount of furnace time. Table 2 gives the cycles for four grades, two cold work steels and two air hardening grades.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:660px;\">\n<thead><tr><th>Steel<\/th><th>Treatment<\/th><\/tr><\/thead>\n<tbody>\n<tr><td class=\"ts-grade\">O1<\/td><td>Heat to 730 &deg;C (1350 &deg;F) and hold for 4 h, heat to 780 &deg;C (1440 &deg;F) and hold for 2 h, cool to 690 &deg;C (1275 &deg;F) and hold for 6 h, then air cool<\/td><\/tr>\n<tr><td class=\"ts-grade\">A2<\/td><td>Heat to 900 &deg;C (1650 &deg;F) and hold for 2 h, cool to 760 &deg;C (1400 &deg;F) and hold for 6 h, then air cool<\/td><\/tr>\n<tr><td class=\"ts-grade\">A6<\/td><td>Heat to 815 &deg;C (1500 &deg;F) and hold for 2 h, cool to 650 &deg;C (1200 &deg;F) and hold for 6 h, then air cool<\/td><\/tr>\n<tr><td class=\"ts-grade\">D2<\/td><td>Heat to 900 &deg;C (1650 &deg;F) and hold for 2 h, cool to 775 &deg;C (1425 &deg;F) and hold for 6 h, then air cool<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 5 of Heat Treating of Specific Classes of Tool Steels. Cycle annealing suits individual tools that can be handled in a liquid bath. The source states that it offers little advantage for large loads.<\/em><\/p> <p class=\"ts-p\">A spheroidize anneal is a hold in a narrow band, and the band is pinned to one transformation line.<\/p>\n<figure class=\"ts-fig\"><img src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg\" alt=\"Temperature range around A1 used for spheroidization, against carbon content, with the intercritical and full annealing bands\" width=\"1156\" height=\"736\" loading=\"lazy\" decoding=\"async\"><figcaption>Fig. 11.11. The temperature range around A<sub>1<\/sub> used for spheroidization, plotted against carbon content, with the intercritical and full annealing bands marked. A hold inside this band, or a cycle that passes through it, turns the lamellar carbide left by normalizing into spheroids and puts the steel in the soft condition a machining operation needs. Holding above the band instead gives a full anneal, which is coarser and harder to finish. Source: E. Essadiqi, Tool Steels, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 11.11.<\/figcaption><\/figure>\n<p class=\"ts-p\">What that hold produces is visible on the microstructure, and it is the structure the annealed stock is sold in.<\/p>\n<figure class=\"ts-fig\"><img src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Annealing-totten-fig-11-12-spheroidized-microstructure-1-percent-c-steel.jpg\" alt=\"Spheroidized microstructure of a 1.0 percent carbon steel at 2000x magnification, globular carbide in a ferrite matrix\" width=\"929\" height=\"910\" loading=\"lazy\" decoding=\"async\"><figcaption>Fig. 11.12. Spheroidized microstructure of a 1.0 % carbon steel at &#215;2000. The carbide is present as globules in a ferrite matrix instead of the lamellar pearlite it replaced, which is the condition a spheroidize anneal is specified to produce before machining and hardening. A structure that looks like this is soft enough to cut and still carries the carbon the hardening step will need. Source: E. Essadiqi, Tool Steels, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 11.12.<\/figcaption><\/figure>\n<h2 class=\"ts-h2\">Heating time to reach the tempering temperature<\/h2>\n<p class=\"ts-p\">A tempering furnace is set to a temperature and the load needs a stated number of minutes per millimetre of section to arrive at it. The allowance depends on the shape of the part and on whether the furnace has forced circulation. Table 3 gives the source figures for a hot air oven without circulation and for a circulating air oven or an oil bath.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:1000px;\">\n<thead><tr><th rowspan=\"3\">Tempering temperature, &deg;C<\/th><th rowspan=\"3\">Tempering temperature, &deg;F<\/th><th colspan=\"6\">Hot air oven without circulation (a)<\/th><th colspan=\"6\">Circulating air oven or an oil bath (b)<\/th><\/tr><tr><th colspan=\"2\">Cubes or spheres<\/th><th colspan=\"2\">Squares or cylinders<\/th><th colspan=\"2\">Average flats<\/th><th colspan=\"2\">Cubes or spheres<\/th><th colspan=\"2\">Squares or cylinders<\/th><th colspan=\"2\">Average flats<\/th><\/tr><tr><th>min\/mm<\/th><th>min\/in.<\/th><th>min\/mm<\/th><th>min\/in.<\/th><th>min\/mm<\/th><th>min\/in.<\/th><th>min\/mm<\/th><th>min\/in.<\/th><th>min\/mm<\/th><th>min\/in.<\/th><th>min\/mm<\/th><th>min\/in.<\/th><\/tr><\/thead>\n<tbody>\n<tr><td class=\"ts-num\">120<\/td><td class=\"ts-num\">250<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><td class=\"ts-num\">2.2<\/td><td class=\"ts-num\">55<\/td><td class=\"ts-num\">3.2<\/td><td class=\"ts-num\">80<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-num\">150<\/td><td class=\"ts-num\">300<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><td class=\"ts-num\">2.0<\/td><td class=\"ts-num\">50<\/td><td class=\"ts-num\">3.0<\/td><td class=\"ts-num\">75<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-num\">175<\/td><td class=\"ts-num\">350<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><td class=\"ts-num\">2.0<\/td><td class=\"ts-num\">50<\/td><td class=\"ts-num\">2.8<\/td><td class=\"ts-num\">70<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-num\">205<\/td><td class=\"ts-num\">400<\/td><td class=\"ts-num\">1.0<\/td><td class=\"ts-num\">25<\/td><td class=\"ts-num\">1.8<\/td><td class=\"ts-num\">45<\/td><td class=\"ts-num\">2.6<\/td><td class=\"ts-num\">65<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-num\">260<\/td><td class=\"ts-num\">500<\/td><td class=\"ts-num\">1.0<\/td><td class=\"ts-num\">25<\/td><td class=\"ts-num\">1.6<\/td><td class=\"ts-num\">40<\/td><td class=\"ts-num\">2.4<\/td><td class=\"ts-num\">60<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-num\">315<\/td><td class=\"ts-num\">600<\/td><td class=\"ts-num\">1.0<\/td><td class=\"ts-num\">25<\/td><td class=\"ts-num\">1.6<\/td><td class=\"ts-num\">40<\/td><td class=\"ts-num\">2.2<\/td><td class=\"ts-num\">55<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-num\">370<\/td><td class=\"ts-num\">700<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.4<\/td><td class=\"ts-num\">35<\/td><td class=\"ts-num\">2.0<\/td><td class=\"ts-num\">50<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-num\">425<\/td><td class=\"ts-num\">800<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><td class=\"ts-num\">1.8<\/td><td class=\"ts-num\">45<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<tr><td class=\"ts-num\">&ge;480<\/td><td class=\"ts-num\">&ge;900<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><td class=\"ts-num\">1.6<\/td><td class=\"ts-num\">40<\/td><td class=\"ts-num\">0.6<\/td><td class=\"ts-num\">15<\/td><td class=\"ts-num\">0.8<\/td><td class=\"ts-num\">20<\/td><td class=\"ts-num\">1.2<\/td><td class=\"ts-num\">30<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 7 of Introduction to Heat Treating of Tool Steels. Data are given in minutes per millimetre, and in minutes per inch, of diameter or thickness, with the furnace held at the temperature in the first column. The source allows the same allowance to be applied to charges of irregular shapes and quantities by estimating the total size of the charge and the number of inches from the outside to the centre of the charge.<\/em><\/p> <h2 class=\"ts-h2\">Automated salt bath lines<\/h2>\n<p class=\"ts-p\">Production heat treating of high speed steel drills, taps and milling cutters is often run on a chain conveyor line with preheat, high heat, quench, wash and rinse stations. The parts travel on tong fixtures, and every station in the line except the air cool is held for one cycle time. Table 4 gives the stage temperatures and the multiples of the cycle time, and Table 5 gives the cycle time for a range of drill diameters and for end mills and cups.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:760px;\">\n<thead><tr><th>Process stage<\/th><th>Operating temperature, &deg;C<\/th><th>Operating temperature, &deg;F<\/th><th>Total time in furnace (a)<\/th><\/tr><\/thead>\n<tbody>\n<tr><td>First preheat<\/td><td class=\"ts-num\">650-870<\/td><td class=\"ts-num\">1200-1600<\/td><td>X<\/td><\/tr>\n<tr><td>Second preheat<\/td><td class=\"ts-num\">760-1040<\/td><td class=\"ts-num\">1400-1900<\/td><td>X<\/td><\/tr>\n<tr><td>High heat<\/td><td class=\"ts-num\">1010-1290<\/td><td class=\"ts-num\">1850-2350<\/td><td>X<\/td><\/tr>\n<tr><td>Isothermal quench<\/td><td class=\"ts-num\">540-705<\/td><td class=\"ts-num\">1000-1300<\/td><td>X<\/td><\/tr>\n<tr><td>Air cool<\/td><td>Room temperature<\/td><td>Room temperature<\/td><td>6X, 12X, 24X<\/td><\/tr>\n<tr><td>Wash, hot water<\/td><td class=\"ts-num\">80-95<\/td><td class=\"ts-num\">180-200<\/td><td>6X<\/td><\/tr>\n<tr><td>Rinse, hot water<\/td><td class=\"ts-num\">80-95<\/td><td class=\"ts-num\">180-200<\/td><td>X<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 2 of Processes and Furnace Equipment for Heat Treating of Tool Steels. X is the cycle time of the line. The source notes that a nitrate quench after the neutral salt quench cuts the air cooling time from 24X to 6X, and warns that as little as 600 ppm of nitrate salts carried into the high heat furnace causes severe surface damage.<\/em><\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:660px;\">\n<thead><tr><th>Drill diameter, mm<\/th><th>Drill diameter, in.<\/th><th rowspan=\"1\">Time<\/th><\/tr><\/thead>\n<tbody>\n<tr><td class=\"ts-num\">2.54-4.78<\/td><td class=\"ts-num\">0.100-0.188<\/td><td>1 min 30 s<\/td><\/tr>\n<tr><td class=\"ts-num\">4.80-8.08<\/td><td class=\"ts-num\">0.189-0.318<\/td><td>1 min 40 s<\/td><\/tr>\n<tr><td class=\"ts-num\">8.10-12.90<\/td><td class=\"ts-num\">0.319-0.508<\/td><td>1 min 50 s<\/td><\/tr>\n<tr><td class=\"ts-num\">12.93-18.24<\/td><td class=\"ts-num\">0.509-0.718<\/td><td>2 min 0 s<\/td><\/tr>\n<tr><td class=\"ts-num\">18.26-23.32<\/td><td class=\"ts-num\">0.719-0.918<\/td><td>2 min 20 s<\/td><\/tr>\n<tr><td class=\"ts-num\">23.34-38.10<\/td><td class=\"ts-num\">0.919-1.500<\/td><td>2 min 40 s<\/td><\/tr>\n<tr><td class=\"ts-num\">102 mm (4 in.) diameter cups<\/td><td><\/td><td>6 min<\/td><\/tr>\n<tr><td class=\"ts-num\">64 mm (2 1\/2 in.) diameter end mills<\/td><td><\/td><td>7 min<\/td><\/tr>\n<tr><td class=\"ts-num\">76 mm (3 in.) diameter end mills<\/td><td><\/td><td>10 min<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 3 of Processes and Furnace Equipment for Heat Treating of Tool Steels. High heat times for the line in Table 4. The same table lists how many pieces of each small diameter are loaded per tong, and the source gives the figures below.<\/em><\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:660px;\">\n<thead><tr><th>Diameter of the pieces in high heat<\/th><th>Load<\/th><\/tr><\/thead>\n<tbody>\n<tr><td>2.54 mm (0.100 in.)<\/td><td>160 pieces per tong, 480 pieces in bath, 1.2 kg (2.6 lb)<\/td><\/tr>\n<tr><td>4.78 mm (0.188 in.)<\/td><td>85 pieces per tong, 255 pieces in bath, 3.5 kg (7.65 lb)<\/td><\/tr>\n<tr><td>6.50 mm (0.256 in.)<\/td><td>63 pieces per tong, 188 pieces in bath, 5.6 kg (12.3 lb)<\/td><\/tr>\n<tr><td>8.08 mm (0.318 in.)<\/td><td>25 pieces per tong, 75 pieces in bath, 3.9 kg (8.6 lb)<\/td><\/tr>\n<tr><td>12.90 mm (0.508 in.)<\/td><td>16 pieces per tong, 48 pieces in bath, 8.3 kg (18.2 lb)<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 3 of Processes and Furnace Equipment for Heat Treating of Tool Steels. Load weights for the small diameters on the automated line.<\/em><\/p> <h2 class=\"ts-h2\">Furnace atmosphere dew point<\/h2>\n<p class=\"ts-p\">Hardening in a controlled atmosphere protects the surface of the tool, and the protection depends on the carbon potential of the gas. For an AGA class 302 endothermic atmosphere the practical control is the dew point. The ranges in Table 7 are quoted for short times at temperature, which suits small tools. The source warns that a large die section needs closer control of the same atmosphere, because the cycle is long enough for a small carbon imbalance at the surface to grow into a carburized or a decarburized case.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:660px;\">\n<thead><tr><th>Steel<\/th><th rowspan=\"2\">Furnace temperature, &deg;C<\/th><th rowspan=\"2\">Furnace temperature, &deg;F<\/th><th colspan=\"2\">Dew point range, &deg;C<\/th><\/tr><tr><th>Dew point, &deg;C<\/th><th>Dew point, &deg;F<\/th><\/tr><\/thead>\n<tbody>\n<tr><td class=\"ts-grade\">W2, W3<\/td><td class=\"ts-num\">800<\/td><td class=\"ts-num\">1475<\/td><td class=\"ts-num\">7 to 13<\/td><td class=\"ts-num\">45 to 55<\/td><\/tr>\n<tr><td class=\"ts-grade\">S1<\/td><td class=\"ts-num\">925<\/td><td class=\"ts-num\">1700<\/td><td class=\"ts-num\">4 to 7<\/td><td class=\"ts-num\">40 to 45<\/td><\/tr>\n<tr><td class=\"ts-grade\">S2<\/td><td class=\"ts-num\">870<\/td><td class=\"ts-num\">1600<\/td><td class=\"ts-num\">4 to 16<\/td><td class=\"ts-num\">40 to 60<\/td><\/tr>\n<tr><td class=\"ts-grade\">O1<\/td><td class=\"ts-num\">800<\/td><td class=\"ts-num\">1475<\/td><td class=\"ts-num\">7 to 12<\/td><td class=\"ts-num\">45 to 55<\/td><\/tr>\n<tr><td class=\"ts-grade\">O2<\/td><td class=\"ts-num\">775<\/td><td class=\"ts-num\">1425<\/td><td class=\"ts-num\">7 to 12<\/td><td class=\"ts-num\">45 to 55<\/td><\/tr>\n<tr><td class=\"ts-grade\">O7<\/td><td class=\"ts-num\">855<\/td><td class=\"ts-num\">1575<\/td><td class=\"ts-num\">-4 to 2<\/td><td class=\"ts-num\">25 to 36<\/td><\/tr>\n<tr><td class=\"ts-grade\">D2, D4<\/td><td class=\"ts-num\">995<\/td><td class=\"ts-num\">1825<\/td><td class=\"ts-num\">-7 to -1<\/td><td class=\"ts-num\">20 to 30<\/td><\/tr>\n<tr><td class=\"ts-grade\">D3, D6<\/td><td class=\"ts-num\">955<\/td><td class=\"ts-num\">1750<\/td><td class=\"ts-num\">-7 to -1<\/td><td class=\"ts-num\">20 to 30<\/td><\/tr>\n<tr><td class=\"ts-grade\">H11, H12, H13<\/td><td class=\"ts-num\">1010<\/td><td class=\"ts-num\">1850<\/td><td class=\"ts-num\">2 to 7<\/td><td class=\"ts-num\">35 to 45<\/td><\/tr>\n<tr><td class=\"ts-grade\">T1<\/td><td class=\"ts-num\">1290<\/td><td class=\"ts-num\">2350<\/td><td class=\"ts-num\">-18 to -12<\/td><td class=\"ts-num\">0 to 10<\/td><\/tr>\n<tr><td class=\"ts-grade\">M1<\/td><td class=\"ts-num\">1205<\/td><td class=\"ts-num\">2200<\/td><td class=\"ts-num\">-15 to -12<\/td><td class=\"ts-num\">5 to 10<\/td><\/tr>\n<tr><td class=\"ts-grade\">F2, F3<\/td><td class=\"ts-num\">830<\/td><td class=\"ts-num\">1525<\/td><td class=\"ts-num\">5 to 1<\/td><td class=\"ts-num\">23 to 34<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 4 of Processes and Furnace Equipment for Heat Treating of Tool Steels. Data compiled for short times at temperature, with furnace dew point quoted for an AGA class 302 endothermic atmosphere. The source prints the Celsius dew point range for F2 and F3 as 5 to 1 while the Fahrenheit range for the same row is 23 to 34, and the two do not agree, so the row is reproduced exactly as printed.<\/em><\/p> <h2 class=\"ts-h2\">Packing compounds for annealing<\/h2>\n<p class=\"ts-p\">When a tool is annealed in a pack, the compound packed around it sets the carbon level at the surface of the steel. Fig. 2 shows the temperature range in which each of the common compounds carburizes, holds a neutral condition or decarburizes the steel. The source notes that the changes from one behaviour to another are gradual, and that the temperature at which used cast iron chips begin to decarburize depends on the carbon content of the chips.<\/p>\n<figure>\n<img src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Heat-Treating-Practices-fig-2-packing-compounds.png\" alt=\"Range of usefulness of packing compounds used in the annealing of tool steels, plotted against temperature in degrees Celsius and degrees Fahrenheit\" width=\"542\" height=\"532\" loading=\"lazy\" decoding=\"async\">\n<figcaption>Fig. 2. Approximate range of usefulness of selected packing compounds used in the annealing of tool steels. Reproduced from the source figure.<\/figcaption>\n<\/figure> <h2 class=\"ts-h2\">What these tables do not fix<\/h2>\n<p class=\"ts-p\">Each table describes the practice of the plant or the source that produced it, so the numbers are a starting point for a process sheet, and the process sheet still has to be written for the tool in hand. Section size, part geometry, the furnace load, the condition of the quench tank and the thermocouple position all move the result. A new tool should have its hardness checked on a first article before the cycle is released to production, and a change of steel supplier is enough reason to check it again. The alloying and the annealed structure of the bar going into the furnace have as much effect on the outcome as the cycle written on the card.<\/p> <p class=\"ts-source\">Source: ASM Handbook, Volume 4, Heat Treating, ASM International, 1991.<\/p> <\/div><\/div><\/div><\/section>\n","protected":false},"excerpt":{"rendered":"<p>Tool Steel | Heat Treating Practice Tool Steel Heat Treating Practices A tool steel performs the way its heat treating cycle prepared it, and most of the tool life that is lost in a shop is lost in the hours between the quench and the final temper. The tables on this page are the published [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20871","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.6 (Yoast SEO v28.6) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Tool Steel Heat Treating Practice Data and Cycles<\/title>\n<meta name=\"description\" content=\"Heat treating practice data for tool steels. Safe delay from quench to temper, cycle annealing schedules, furnace heat up times to the tempering temperature, automated salt bath line cycles and endothermic atmosphere dew point ranges.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treating-practices\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Tool Steel Heat Treating Practices\" \/>\n<meta property=\"og:description\" content=\"Heat treating practice data for tool steels. Safe delay from quench to temper, cycle annealing schedules, furnace heat up times to the tempering temperature, automated salt bath line cycles and endothermic atmosphere dew point ranges.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treating-practices\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-10T15:39:07+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"9\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Tool Steel Heat Treating Practices\",\"datePublished\":\"2026-10-03T23:21:27+00:00\",\"dateModified\":\"2026-10-10T15:39:07+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/\"},\"wordCount\":1856,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg\",\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/\",\"name\":\"Tool Steel Heat Treating Practice Data and Cycles\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg\",\"datePublished\":\"2026-10-03T23:21:27+00:00\",\"dateModified\":\"2026-10-10T15:39:07+00:00\",\"description\":\"Heat treating practice data for tool steels. Safe delay from quench to temper, cycle annealing schedules, furnace heat up times to the tempering temperature, automated salt bath line cycles and endothermic atmosphere dew point ranges.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treating-practices\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Tool Steel Heat Treating Practices\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tool Steel Heat Treating Practice Data and Cycles","description":"Heat treating practice data for tool steels. Safe delay from quench to temper, cycle annealing schedules, furnace heat up times to the tempering temperature, automated salt bath line cycles and endothermic atmosphere dew point ranges.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treating-practices\/","og_locale":"ko_KR","og_type":"article","og_title":"Tool Steel Heat Treating Practices","og_description":"Heat treating practice data for tool steels. Safe delay from quench to temper, cycle annealing schedules, furnace heat up times to the tempering temperature, automated salt bath line cycles and endothermic atmosphere dew point ranges.","og_url":"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treating-practices\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-10T15:39:07+00:00","og_image":[{"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"9\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Tool Steel Heat Treating Practices","datePublished":"2026-10-03T23:21:27+00:00","dateModified":"2026-10-10T15:39:07+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/"},"wordCount":1856,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg","inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/","url":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/","name":"Tool Steel Heat Treating Practice Data and Cycles","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg","datePublished":"2026-10-03T23:21:27+00:00","dateModified":"2026-10-10T15:39:07+00:00","description":"Heat treating practice data for tool steels. Safe delay from quench to temper, cycle annealing schedules, furnace heat up times to the tempering temperature, automated salt bath line cycles and endothermic atmosphere dew point ranges.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/"]}]},{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Annealing-totten-fig-11-11-spheroidization-temperature-range-around-a1.jpg"},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-heat-treating-practices\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Tool Steel Heat Treating Practices"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tool Steel | Heat Treating Practice Tool Steel Heat Treating Practices A tool steel performs the way its heat treating cycle prepared it, and most of the tool life that is lost in a shop is lost in the hours between the quench and the final temper. The tables on this page are the published&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tool Steel | Heat Treating Practice Tool Steel Heat Treating Practices A tool steel performs the way its heat treating cycle prepared it, and most of the tool life that is lost in a shop is lost in the hours between the quench and the final temper. The tables on this page are the published&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20871","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20871"}],"version-history":[{"count":6,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20871\/revisions"}],"predecessor-version":[{"id":21742,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20871\/revisions\/21742"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20871"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}