{"id":20826,"date":"2026-10-03T16:45:04","date_gmt":"2026-10-03T08:45:04","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20826"},"modified":"2026-10-16T16:07:21","modified_gmt":"2026-10-16T08:07:21","slug":"l-series-s-series-tool-steel-properties","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/l-series-s-series-tool-steel-properties\/","title":{"rendered":"L \uc2dc\ub9ac\uc988 \ubc0f S \uc2dc\ub9ac\uc988 \uacf5\uad6c\uac15 \ud2b9\uc131, \uc5b4\ub2d0\ub9c1 \ubc0f \uacbd\ud654"},"content":{"rendered":"<h1 class=\"wp-block-heading\">L \uc2dc\ub9ac\uc988 \ubc0f S \uc2dc\ub9ac\uc988 \uacf5\uad6c\uac15 \ud2b9\uc131, \uc5b4\ub2d0\ub9c1 \ubc0f \uacbd\ud654<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">L \uc2dc\ub9ac\uc988\uc640 S \uc2dc\ub9ac\uc988\ub294 \ub0b4\ub9c8\ubaa8\uc131\uc774\ub098 \uace0\uc628 \uacbd\ub3c4\ubcf4\ub2e4\ub294 \uac15\ub3c4\uc640 \ub0b4\ucda9\uaca9\uc131\uc744 \uc704\ud574 \uad6c\ub9e4\ub418\ub294 \ub450 \uac00\uc9c0 \uacf5\uad6c\uac15 \uadf8\ub8f9\uc785\ub2c8\ub2e4. L\uc740 \uc800\ud569\uae08 \ud2b9\uc218 \ubaa9\uc801 \uadf8\ub8f9\uc774\uace0, S\ub294 \ub0b4\ucda9\uaca9 \uadf8\ub8f9\uc774\uba70, \ub458 \ub2e4 \ub9c8\ucc30\ubcf4\ub2e4\ub294 \ucda9\uaca9\uc744 \ubc1b\ub294 \ubd80\ud488\uc5d0 \uc0ac\uc6a9\ub429\ub2c8\ub2e4: \uc815, \ud380\uce58, \ub9ac\ubcb3 \uc138\ud2b8, \uc804\ub2e8 \ub0a0, \uc544\ubc84, \ucea0, \ucc99 \ubc0f \ucf5c\ub9bf. \uc774 \ud398\uc774\uc9c0\ub294 \ud604\uc7ac \uc0c1\uc5c5\uc801\uc73c\ub85c \uc0ac\uc6a9\ub418\ub294 \ub4f1\uae09\uc758 \uacf5\ud45c\ub41c \uae30\uacc4\uc801 \ud2b9\uc131\uc744 \uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc \ubc0f \uac01 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uc5d0\uc11c \uc81c\uacf5\ud558\ubbc0\ub85c, \uc791\uc5c5\uc5d0 \ud544\uc694\ud55c \uacbd\ub3c4\uc5d0\uc11c\uc758 \uac15\ub3c4\uc640 \uc778\uc131\uc744 \ud568\uaed8 \ud655\uc778\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">L \uadf8\ub8f9, \uc800\ud569\uae08 \ud2b9\uc218 \ubaa9\uc801 \uac15<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">L \uadf8\ub8f9 \uac15\uc740 \uc18c\ub7c9\uc758 \ud06c\ub86c, \ubc14\ub098\ub4d0, \ub2c8\ucf08 \ubc0f \ubab0\ub9ac\ube0c\ub374\uc744 \ud568\uc720\ud558\uba70, \uc774 \uadf8\ub8f9\uc5d0\ub294 \ud55c\ub54c 7\uac1c\uc758 \ub4f1\uae09\uc774 \uc788\uc5c8\uc2b5\ub2c8\ub2e4. <a href=\"https:\/\/aobosteel.com\/ko\/obsolete-tool-steel-grades\/\">L2\uc640 L6 \ub450 \uac00\uc9c0 \ub9cc\uc774 \ub0a8\uc544 \uc788\uc2b5\ub2c8\ub2e4<\/a>. L2\ub294 0.50~1.10%\uc758 \uc5ec\ub7ec \ud0c4\uc18c \ud568\ub7c9\uc73c\ub85c \uc81c\uacf5\ub418\uba70, \ud06c\ub86c\uacfc \ubc14\ub098\ub4d0\uc73c\ub85c \uc778\ud574 \ubbf8\uc138 \uacb0\uc815\ub9bd\uc758 \uc720\ub0c9 \uacbd\ud654\uac15\uc785\ub2c8\ub2e4. L6\ub294 \uc778\uc131\uc744 \uc704\ud574 \uc57d 1.50%\uc758 \ub2c8\ucf08\uc744 \ucca8\uac00\ud569\ub2c8\ub2e4. \ub458 \ub2e4 \uba85\ubaa9\uc0c1 \uc720\ub0c9 \uacbd\ud654\uc774\uc9c0\ub9cc, \uc2e4\uc81c\ub85c\ub294 \ud070 L2 \ub2e8\uba74\uc740 \uc885\uc885 \ub300\uc2e0 \uc218\ub0c9\ub429\ub2c8\ub2e4. \uadf8\ub8f9 \ub0b4 \uacbd\ud654\ub2a5 \ubc94\uc704\ub294 \ub113\uc73c\uba70, \uc774\ub294 \ud569\uae08 \ud6a8\uacfc\ub9cc\ud07c \ud0c4\uc18c \ud6a8\uacfc\uc774\uae30\ub3c4 \ud569\ub2c8\ub2e4: \ud0c4\uc18c 0.50%\uc758 L2\ub294 \uc720\ub0c9 \uc2dc \uc57d 57 HRC\uc5d0 \ub3c4\ub2ec\ud558\uc9c0\ub9cc \uc57d 12.7 mm \uc774\uc0c1\uc758 \ub2e8\uba74\uc5d0\uc11c\ub294 \uc644\uc804 \uacbd\ud654\ub418\uc9c0 \uc54a\ub294 \ubc18\uba74, \ud0c4\uc18c 0.70%\uc758 L6\ub294 \ub0c9\uac01 \uc2dc \uc57d 64 HRC\uc5d0 \ub3c4\ub2ec\ud558\uace0 76 mm\uae4c\uc9c0 60 HRC \uc774\uc0c1\uc744 \uc720\uc9c0\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 7. L2, \uc0c1\uc628 \uacf5\uce6d \uae30\uacc4\uc801 \ud2b9\uc131<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\ud0dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc2e0\uc728, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \uc218\ucd95\ub960, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, J<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, ft&#183;lbf<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">855 &#176;C (1575 &#176;F)\uc5d0\uc11c \uc720\ub0c9 \ud6c4 \ub2e8\uc77c \ud15c\ud37c\ub9c1:<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">710<\/td><td class=\"has-text-align-left\" data-align=\"left\">103<\/td><td class=\"has-text-align-left\" data-align=\"left\">510<\/td><td class=\"has-text-align-left\" data-align=\"left\">74<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">205 &#176;C (400 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">290<\/td><td class=\"has-text-align-left\" data-align=\"left\">1790<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><td class=\"has-text-align-left\" data-align=\"left\">28<\/td><td class=\"has-text-align-left\" data-align=\"left\">21<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">315 &#176;C (600 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1790<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">1655<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">19<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">425 &#176;C (800 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">225<\/td><td class=\"has-text-align-left\" data-align=\"left\">1380<\/td><td class=\"has-text-align-left\" data-align=\"left\">200<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">47<\/td><td class=\"has-text-align-left\" data-align=\"left\">26<\/td><td class=\"has-text-align-left\" data-align=\"left\">19<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">540 &#176;C (1000 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1275<\/td><td class=\"has-text-align-left\" data-align=\"left\">185<\/td><td class=\"has-text-align-left\" data-align=\"left\">1170<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">41<\/td><td class=\"has-text-align-left\" data-align=\"left\">39<\/td><td class=\"has-text-align-left\" data-align=\"left\">29<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">650 &#176;C (1200 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">930<\/td><td class=\"has-text-align-left\" data-align=\"left\">135<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">92<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 7. L6, \uc0c1\uc628 \uacf5\uce6d \uae30\uacc4\uc801 \ud2b9\uc131<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\ud0dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc2e0\uc728, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \uc218\ucd95\ub960, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, J<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, ft&#183;lbf<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">845 &#176;C (1550 &#176;F)\uc5d0\uc11c \uc720\ub0c9 \ud6c4 \ub2e8\uc77c \ud15c\ud37c\ub9c1:<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">655<\/td><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">93 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">315 &#176;C (600 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">290<\/td><td class=\"has-text-align-left\" data-align=\"left\">1790<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">425 &#176;C (800 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1585<\/td><td class=\"has-text-align-left\" data-align=\"left\">230<\/td><td class=\"has-text-align-left\" data-align=\"left\">1380<\/td><td class=\"has-text-align-left\" data-align=\"left\">200<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">46<\/td><td class=\"has-text-align-left\" data-align=\"left\">18<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">540 &#176;C (1000 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1345<\/td><td class=\"has-text-align-left\" data-align=\"left\">195<\/td><td class=\"has-text-align-left\" data-align=\"left\">1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">160<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">42<\/td><td class=\"has-text-align-left\" data-align=\"left\">23<\/td><td class=\"has-text-align-left\" data-align=\"left\">17<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">650 &#176;C (1200 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">965<\/td><td class=\"has-text-align-left\" data-align=\"left\">140<\/td><td class=\"has-text-align-left\" data-align=\"left\">830<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">32<\/td><td class=\"has-text-align-left\" data-align=\"left\">81<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98: ASM Handbook Vol.1, Wrought Tool Steels \ud56d\ubaa9, Table 7. \uc5b4\ub2d0\ub9c1\ub41c \ud589\uc740 \uacf5\uae09 \uc0c1\ud0dc(as-supplied condition)\ub97c \ub098\ud0c0\ub0c5\ub2c8\ub2e4. \ucd9c\ucc98 \uac01\uc8fc: (a) \uc5f0\uc2e0\uc728\uc740 50 mm (2 in.) \uac8c\uc774\uc9c0 \uae38\uc774\uc5d0\uc11c \uce21\uc815, (b) Charpy V-\ub178\uce58, (c) Charpy \ubb34\ub178\uce58. L \ub4f1\uae09\uc740 \ub178\uce58 \uc2dc\ud5d8 \uae30\uc900\uc73c\ub85c, S \ub4f1\uae09\uc740 \ubb34\ub178\uce58 \uc2dc\ud5d8 \uae30\uc900\uc73c\ub85c \uc81c\uc2dc\ub418\uc5b4 \uc788\uc73c\ubbc0\ub85c \ub450 \uadf8\ub8f9\uc758 \ucda9\uaca9 \uc5f4\uc740 \uc11c\ub85c \ube44\uad50\ud560 \uc218 \uc5c6\uc2b5\ub2c8\ub2e4. \ub300\uc2dc(-)\ub294 \ucd9c\ucc98\uc5d0 \uac12\uc774 \uc5c6\uc74c\uc744 \uc758\ubbf8\ud569\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">S \uadf8\ub8f9, \ub0b4\ucda9\uaca9 \uac15<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">S \uadf8\ub8f9 \uac15\uc740 \uacf5\uad6c\uac00 \ucda9\uaca9\uc744 \ud761\uc218\ud574\uc57c \ud560 \ub54c \uc9c0\uc815\ub418\ub294 \uac15\uc785\ub2c8\ub2e4. \uc774\ub4e4\uc740 \uc595\uc740 \uacbd\ud654(S2)\uc5d0\uc11c \uae4a\uc740 \uacbd\ud654(S7)\uae4c\uc9c0 \ub2e4\uc591\ud558\uba70, \uc5ec\uae30\uc11c \uacbd\ud654\ub2a5\uc740 W \uadf8\ub8f9\uc744 \uc9c0\ubc30\ud558\ub294 \uacb0\uc815\ub9bd \ud06c\uae30 \ubc0f \uc6a9\ud574 \uacf5\uc815 \ud6a8\uacfc\ubcf4\ub2e4\ub294 \uc870\uc131\uc5d0 \uc758\ud574 \uc81c\uc5b4\ub429\ub2c8\ub2e4. \uc774 \uadf8\ub8f9\uc740 \ucd5c\uc801 \uacbd\ub3c4\uc5d0 \ub3c4\ub2ec\ud558\uae30 \uc704\ud574 \uc0c1\ub300\uc801\uc73c\ub85c \ub192\uc740 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4\uac00 \ud544\uc694\ud558\uba70, \uadf8\ub85c \uc778\ud574 \ubbf8\uc6a9\ud574 \ud0c4\ud654\ubb3c\uc774 \ub2e4\ub978 \uadf8\ub8f9\uc5d0\uc11c\ucc98\ub7fc \uacbd\ud654\ub2a5 \uc81c\uc5b4 \uc694\uc18c\uac00 \uc544\ub2d9\ub2c8\ub2e4. S2\ub294 \uc77c\ubc18\uc801\uc73c\ub85c \uc218\ub0c9\ub418\uace0, S1, S5 \ubc0f S6\ub294 \uc720\ub0c9\ub418\uba70, S7\uc740 \ud070 \ub2e8\uba74\uc744 \uc81c\uc678\ud558\uace0 \uc77c\ubc18\uc801\uc73c\ub85c \uacf5\ub0c9\ub418\uba70, \ud070 \ub2e8\uba74\uc740 \uc720\ub0c9\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \ud45c\uc5d0 \uc788\ub294 \uc138 \ub4f1\uae09\uc758 \uae30\uacc4\uc801 \ud2b9\uc131\uc740 S \uadf8\ub8f9\uc774 \ub54c\ub54c\ub85c \ube44\uacf5\uad6c \uc791\uc5c5\uc5d0 \uace0\ub824\ub418\ub294 \uc774\uc720\uc785\ub2c8\ub2e4. 205 &#176;C (400 &#176;F) \ud15c\ud37c\uc5d0\uc11c S5\ub294 2345 MPa (340 ksi) \uc778\uc7a5\uac15\ub3c4\uc640 206 J\uc758 \ubb34\ub178\uce58 \ucda9\uaca9 \uc5d0\ub108\uc9c0\uc5d0 \ub3c4\ub2ec\ud558\uba70, S7\uc740 650 &#176;C (1200 &#176;F) \ud15c\ud37c\uc5d0\uc11c 358 J\uc5d0 \ub3c4\ub2ec\ud558\uba74\uc11c\ub3c4 1240 MPa (180 ksi)\ub97c \uc720\uc9c0\ud569\ub2c8\ub2e4. \uac15\ub3c4\uc640 \uc778\uc131\uc740 \uacf5\uad6c\uac15\uc5d0\uc11c \ud754\uce58 \uc54a\uc740 \ubc29\uc2dd\uc73c\ub85c \ud15c\ud37c\ub9c1 \ubc94\uc704 \uc804\ubc18\uc5d0 \uac78\uccd0 \ud568\uaed8 \uc6c0\uc9c1\uc774\uba70, 650 &#176;C \ud589\uc5d0\uc11c \uc774\uac83\uc774 \uac00\uc7a5 \uba85\ud655\ud558\uac8c \ub098\ud0c0\ub0a9\ub2c8\ub2e4: \uacbd\ub3c4\ub294 30\ub300 \ud6c4\ubc18\uc73c\ub85c \ub5a8\uc5b4\uc9c0\uace0 \ucda9\uaca9 \uc5d0\ub108\uc9c0\ub294 \uc57d \ud55c \uc790\ub9bf\uc218 \uc99d\uac00\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 7. S1, \uc0c1\uc628 \uacf5\uce6d \uae30\uacc4\uc801 \ud2b9\uc131<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\ud0dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc2e0\uc728, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \uc218\ucd95\ub960, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, J<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, ft&#183;lbf<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">925 &#176;C (1700 &#176;F)\uc5d0\uc11c \uc720\ub0c9 \ud6c4 \ub2e8\uc77c \ud15c\ud37c\ub9c1:<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">415<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">24<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">205 &#176;C (400 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2070<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">1895<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">249<\/td><td class=\"has-text-align-left\" data-align=\"left\">184<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">315 &#176;C (600 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2025<\/td><td class=\"has-text-align-left\" data-align=\"left\">294<\/td><td class=\"has-text-align-left\" data-align=\"left\">1860<\/td><td class=\"has-text-align-left\" data-align=\"left\">270<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><td class=\"has-text-align-left\" data-align=\"left\">233<\/td><td class=\"has-text-align-left\" data-align=\"left\">172<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">425 &#176;C (800 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1790<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">1690<\/td><td class=\"has-text-align-left\" data-align=\"left\">245<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">17<\/td><td class=\"has-text-align-left\" data-align=\"left\">50.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">203<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">540 &#176;C (1000 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1680<\/td><td class=\"has-text-align-left\" data-align=\"left\">244<\/td><td class=\"has-text-align-left\" data-align=\"left\">1525<\/td><td class=\"has-text-align-left\" data-align=\"left\">221<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><td class=\"has-text-align-left\" data-align=\"left\">23<\/td><td class=\"has-text-align-left\" data-align=\"left\">47.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">230<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">650 &#176;C (1200 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1345<\/td><td class=\"has-text-align-left\" data-align=\"left\">195<\/td><td class=\"has-text-align-left\" data-align=\"left\">1240<\/td><td class=\"has-text-align-left\" data-align=\"left\">180<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">37<\/td><td class=\"has-text-align-left\" data-align=\"left\">42<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 7. S5, \uc0c1\uc628 \uacf5\uce6d \uae30\uacc4\uc801 \ud2b9\uc131<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\ud0dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc2e0\uc728, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \uc218\ucd95\ub960, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, J<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, ft&#183;lbf<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">870 &#176;C (1600 &#176;F)\uc5d0\uc11c \uc720\ub0c9 \ud6c4 \ub2e8\uc77c \ud15c\ud37c\ub9c1:<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">725<\/td><td class=\"has-text-align-left\" data-align=\"left\">105<\/td><td class=\"has-text-align-left\" data-align=\"left\">440<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">205 &#176;C (400 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2345<\/td><td class=\"has-text-align-left\" data-align=\"left\">340<\/td><td class=\"has-text-align-left\" data-align=\"left\">1930<\/td><td class=\"has-text-align-left\" data-align=\"left\">280<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">59<\/td><td class=\"has-text-align-left\" data-align=\"left\">206<\/td><td class=\"has-text-align-left\" data-align=\"left\">152<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">315 &#176;C (600 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2240<\/td><td class=\"has-text-align-left\" data-align=\"left\">325<\/td><td class=\"has-text-align-left\" data-align=\"left\">1860<\/td><td class=\"has-text-align-left\" data-align=\"left\">270<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">24<\/td><td class=\"has-text-align-left\" data-align=\"left\">58<\/td><td class=\"has-text-align-left\" data-align=\"left\">232<\/td><td class=\"has-text-align-left\" data-align=\"left\">171<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">425 &#176;C (800 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1895<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">1690<\/td><td class=\"has-text-align-left\" data-align=\"left\">245<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><td class=\"has-text-align-left\" data-align=\"left\">28<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">243<\/td><td class=\"has-text-align-left\" data-align=\"left\">179<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">540 &#176;C (1000 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1515<\/td><td class=\"has-text-align-left\" data-align=\"left\">220<\/td><td class=\"has-text-align-left\" data-align=\"left\">1380<\/td><td class=\"has-text-align-left\" data-align=\"left\">200<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">188<\/td><td class=\"has-text-align-left\" data-align=\"left\">139<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">650 &#176;C (1200 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1035<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">1170<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">37<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 7. S7, \uc0c1\uc628 \uacf5\uce6d \uae30\uacc4\uc801 \ud2b9\uc131<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\ud0dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc2e0\uc728, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \uc218\ucd95\ub960, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, J<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9, ft&#183;lbf<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">940 &#176;C (1725 &#176;F)\uc5d0\uc11c \ud32c \ub0c9\uac01 \ud6c4 \ub2e8\uc77c \ud15c\ud37c\ub9c1:<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">640<\/td><td class=\"has-text-align-left\" data-align=\"left\">93<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">205 &#176;C (400 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2170<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">58<\/td><td class=\"has-text-align-left\" data-align=\"left\">244<\/td><td class=\"has-text-align-left\" data-align=\"left\">180<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">315 &#176;C (600 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1965<\/td><td class=\"has-text-align-left\" data-align=\"left\">285<\/td><td class=\"has-text-align-left\" data-align=\"left\">1585<\/td><td class=\"has-text-align-left\" data-align=\"left\">230<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">309<\/td><td class=\"has-text-align-left\" data-align=\"left\">228<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">425 &#176;C (800 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1895<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">1410<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">29<\/td><td class=\"has-text-align-left\" data-align=\"left\">53<\/td><td class=\"has-text-align-left\" data-align=\"left\">243<\/td><td class=\"has-text-align-left\" data-align=\"left\">179<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">540 &#176;C (1000 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1820<\/td><td class=\"has-text-align-left\" data-align=\"left\">264<\/td><td class=\"has-text-align-left\" data-align=\"left\">1380<\/td><td class=\"has-text-align-left\" data-align=\"left\">200<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">33<\/td><td class=\"has-text-align-left\" data-align=\"left\">51<\/td><td class=\"has-text-align-left\" data-align=\"left\">324<\/td><td class=\"has-text-align-left\" data-align=\"left\">239<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">650 &#176;C (1200 &#176;F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1240<\/td><td class=\"has-text-align-left\" data-align=\"left\">180<\/td><td class=\"has-text-align-left\" data-align=\"left\">1035<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">39<\/td><td class=\"has-text-align-left\" data-align=\"left\">358<\/td><td class=\"has-text-align-left\" data-align=\"left\">264<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98: ASM Handbook Vol.1, Wrought Tool Steels \ud56d\ubaa9, Table 7. \uc5b4\ub2d0\ub9c1\ub41c \ud589\uc740 \uacf5\uae09 \uc0c1\ud0dc(as-supplied condition)\ub97c \ub098\ud0c0\ub0c5\ub2c8\ub2e4. \ucd9c\ucc98 \uac01\uc8fc: (a) \uc5f0\uc2e0\uc728\uc740 50 mm (2 in.) \uac8c\uc774\uc9c0 \uae38\uc774\uc5d0\uc11c \uce21\uc815, (b) Charpy V-\ub178\uce58, (c) Charpy \ubb34\ub178\uce58. L \ub4f1\uae09\uc740 \ub178\uce58 \uc2dc\ud5d8 \uae30\uc900\uc73c\ub85c, S \ub4f1\uae09\uc740 \ubb34\ub178\uce58 \uc2dc\ud5d8 \uae30\uc900\uc73c\ub85c \uc81c\uc2dc\ub418\uc5b4 \uc788\uc73c\ubbc0\ub85c \ub450 \uadf8\ub8f9\uc758 \ucda9\uaca9 \uc5f4\uc740 \uc11c\ub85c \ube44\uad50\ud560 \uc218 \uc5c6\uc2b5\ub2c8\ub2e4. \ub300\uc2dc(-)\ub294 \ucd9c\ucc98\uc5d0 \uac12\uc774 \uc5c6\uc74c\uc744 \uc758\ubbf8\ud569\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub450 \ud45c\ub97c \ud568\uaed8 \uc77d\uae30<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \uc218\uce58\uc640 \uad00\ub828\ud558\uc5ec \uc138 \uac00\uc9c0 \uc8fc\uc758 \uc0ac\ud56d\uc774 \uc788\uc2b5\ub2c8\ub2e4. \uccab\uc9f8\ub294 \ucd9c\ucc98 \uac01\uc8fc\uc5d0\uc11c \uc774\ubbf8 \uc5b8\uae09\ud55c \uac83\uc73c\ub85c, L \ub4f1\uae09\uc740 \uc0e4\ub974\ud53c V-\ub178\uce58 \uc2dc\ud5d8\uc73c\ub85c, S \ub4f1\uae09\uc740 \ubb34\ub178\uce58 \uc2dc\ud5d8\uc73c\ub85c \uc778\uc6a9\ub418\ubbc0\ub85c \ud55c \ud45c\uc758 \ucda9\uaca9 \uc218\uce58\ub294 \ub2e4\ub978 \ud45c\uc758 \uc218\uce58\uc640 \ube44\uad50\ud560 \uc218 \uc5c6\uc2b5\ub2c8\ub2e4. \ub458\uc9f8\ub294 \ubaa8\ub4e0 \uac12\uc774 \ub2e8\uc77c \ucd9c\ucc98\uc758 \uc0c1\uc628 \uacf5\uce6d \uac12\uc774\uba70, \uac15\ub3c4\uc640 \uc5f0\uc2e0\uc728\uc740 \ub2e8\uba74 \ud06c\uae30, \uc2e4\uc81c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4 \ubc0f \ud15c\ud37c\ub9c1 \ud69f\uc218\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9c0\ub294\ub370, \uc774 \uc911 \uc5b4\ub290 \uac83\ub3c4 \ud45c \ubcc0\uc218\uc5d0 \ud3ec\ud568\ub418\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \uc14b\uc9f8\ub294 \uc5b4\ub2d0\ub9c1 \ud589\uc758 \uacbd\ub3c4 \uc218\uce58\ub294 \ub85c\ud06c\uc6f0 B \uc2a4\ucf00\uc77c\uc774\uace0 \uacbd\ud654 \ud589\uc740 \ub85c\ud06c\uc6f0 C \uc2a4\ucf00\uc77c\uc774\ubbc0\ub85c, \uc5b4\ub2d0\ub9c1 \uacbd\ub3c4\ub294 \uc791\uc5c5 \uacbd\ub3c4\uac00 \uc544\ub2c8\ub77c \uac00\uacf5\uc131 \uc9c0\ud45c\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc2a4\ucf00\uc77c \uac04 \ubcc0\ud658, \uadf8\ub9ac\uace0 96 HRB \uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc\uc640 54 HRC \uc791\uc5c5 \uc0c1\ud0dc\ub97c \uc9c1\uc811 \ube44\uad50\ud560 \uc218 \uc5c6\ub294 \uc774\uc720\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/vickers-to-rockwell-hardness-conversion\/\">\ube44\ucee4\uc2a4-\ub85c\ud06c\uc6f0 C \ubcc0\ud658<\/a> \ud398\uc774\uc9c0\uc5d0 \uc788\uc2b5\ub2c8\ub2e4. W \uadf8\ub8f9 \ubc0f O \uadf8\ub8f9 \ud2b9\uc131\uc740 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-properties-chart\/\">\uacf5\uad6c\uac15 \ud2b9\uc131 \ucc28\ud2b8<\/a>\uc5d0, \uc774\ub4e4 \uac01 \ub4f1\uae09\uc774 \uc628\ub3c4\uc5d0\uc11c \uc720\uc9c0\ud558\ub294 \uacbd\ub3c4\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-hot-hardness-chart\/\">\uacf5\uad6c\uac15 \uace0\uc628 \uacbd\ub3c4 \ucc28\ud2b8<\/a>\uc5d0, \uadf8\ub9ac\uace0 \uc804\uccb4 \uacc4\uc5f4\uc758 \ucda9\uaca9 \uc5d0\ub108\uc9c0\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-impact-toughness-chart\/\">\uacf5\uad6c\uac15 \ucda9\uaca9 \uc778\uc131 \ucc28\ud2b8<\/a>\uc5d0 \uc788\uc2b5\ub2c8\ub2e4. Aobo Steel\uc740 L6 \ubc0f S7\uc744 \ub2e8\uc870 \ubc0f \uc5f4\uac04 \uc555\uc5f0 \ubd09\uc7ac\ub85c \uacf5\uae09\ud558\uba70, \ubc00 \uc2dc\ud2b8\uc758 \uc5b4\ub2d0\ub9c1 \uacbd\ub3c4\ub294 \ub3d9\uc77c\ud55c \ud45c\ub97c \ub530\ub985\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Vol 1, Properties and Selection: Irons, Steels and High-Performance Alloys.<\/p>","protected":false},"excerpt":{"rendered":"<p>L Series and S Series Tool Steel Properties, Annealed and Hardened The L series and the S series are the two tool steel groups that are bought for strength and shock resistance rather than for wear resistance or hot hardness. L is the low alloy special purpose group, and S is the shock resisting group, [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20826","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>L Series and S Series Tool Steel Properties<\/title>\n<meta name=\"description\" content=\"Nominal room temperature mechanical properties for L2, L6, S1, S5 and S7 tool steel, annealed and at each tempering temperature, with tensile, yield and impact values.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/l-series-s-series-tool-steel-properties\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"L Series and S Series Tool Steel Properties, Annealed and Hardened\" \/>\n<meta property=\"og:description\" content=\"Nominal room temperature mechanical properties for L2, L6, S1, S5 and S7 tool steel, annealed and at each tempering temperature, with tensile, yield and impact values.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/l-series-s-series-tool-steel-properties\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-16T08:07:21+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"5\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/l-series-s-series-tool-steel-properties\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/l-series-s-series-tool-steel-properties\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"L Series and S Series Tool Steel Properties, Annealed and Hardened\",\"datePublished\":\"2026-10-03T08:45:04+00:00\",\"dateModified\":\"2026-10-16T08:07:21+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/l-series-s-series-tool-steel-properties\\\/\"},\"wordCount\":1106,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/l-series-s-series-tool-steel-properties\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/l-series-s-series-tool-steel-properties\\\/\",\"name\":\"L Series and S Series Tool Steel Properties\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-03T08:45:04+00:00\",\"dateModified\":\"2026-10-16T08:07:21+00:00\",\"description\":\"Nominal room temperature mechanical properties for L2, L6, S1, S5 and S7 tool steel, annealed and at each tempering temperature, with tensile, yield and impact values.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/l-series-s-series-tool-steel-properties\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/l-series-s-series-tool-steel-properties\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/l-series-s-series-tool-steel-properties\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"L Series and S Series Tool Steel Properties, Annealed and Hardened\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"L \uacc4\uc5f4 \ubc0f S \uacc4\uc5f4 \uacf5\uad6c\uac15 \ud2b9\uc131","description":"L2, L6, S1, S5 \ubc0f S7 \uacf5\uad6c\uac15\uc758 \uc0c1\uc628 \uacf5\uce6d \uae30\uacc4\uc801 \uc131\uc9c8\uc744 \uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc \ubc0f \uac01 \ud15c\ud37c\ub9c1 \uc628\ub3c4\ubcc4\ub85c \uc778\uc7a5, \ud56d\ubcf5 \ubc0f \ucda9\uaca9 \uac12\uacfc \ud568\uaed8 \uc81c\uc2dc\ud569\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/l-series-s-series-tool-steel-properties\/","og_locale":"ko_KR","og_type":"article","og_title":"L Series and S Series Tool Steel Properties, Annealed and Hardened","og_description":"Nominal room temperature mechanical properties for L2, L6, S1, S5 and S7 tool steel, annealed and at each tempering temperature, with tensile, yield and impact values.","og_url":"https:\/\/aobosteel.com\/ko\/l-series-s-series-tool-steel-properties\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-16T08:07:21+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"5\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/l-series-s-series-tool-steel-properties\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/l-series-s-series-tool-steel-properties\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"L Series and S Series Tool Steel Properties, Annealed and Hardened","datePublished":"2026-10-03T08:45:04+00:00","dateModified":"2026-10-16T08:07:21+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/l-series-s-series-tool-steel-properties\/"},"wordCount":1106,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/l-series-s-series-tool-steel-properties\/","url":"https:\/\/aobosteel.com\/l-series-s-series-tool-steel-properties\/","name":"L \uacc4\uc5f4 \ubc0f S \uacc4\uc5f4 \uacf5\uad6c\uac15 \ud2b9\uc131","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-03T08:45:04+00:00","dateModified":"2026-10-16T08:07:21+00:00","description":"L2, L6, S1, S5 \ubc0f S7 \uacf5\uad6c\uac15\uc758 \uc0c1\uc628 \uacf5\uce6d \uae30\uacc4\uc801 \uc131\uc9c8\uc744 \uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc \ubc0f \uac01 \ud15c\ud37c\ub9c1 \uc628\ub3c4\ubcc4\ub85c \uc778\uc7a5, \ud56d\ubcf5 \ubc0f \ucda9\uaca9 \uac12\uacfc \ud568\uaed8 \uc81c\uc2dc\ud569\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/l-series-s-series-tool-steel-properties\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/l-series-s-series-tool-steel-properties\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/l-series-s-series-tool-steel-properties\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"L Series and S Series Tool Steel Properties, Annealed and Hardened"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"L Series and S Series Tool Steel Properties, Annealed and Hardened The L series and the S series are the two tool steel groups that are bought for strength and shock resistance rather than for wear resistance or hot hardness. L is the low alloy special purpose group, and S is the shock resisting group,&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"L Series and S Series Tool Steel Properties, Annealed and Hardened The L series and the S series are the two tool steel groups that are bought for strength and shock resistance rather than for wear resistance or hot hardness. L is the low alloy special purpose group, and S is the shock resisting group,&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20826","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20826"}],"version-history":[{"count":5,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20826\/revisions"}],"predecessor-version":[{"id":23182,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20826\/revisions\/23182"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20826"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}