{"id":20812,"date":"2026-10-03T16:30:48","date_gmt":"2026-10-03T08:30:48","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20812"},"modified":"2026-10-16T01:16:22","modified_gmt":"2026-10-15T17:16:22","slug":"cpm-high-speed-steel-test-data","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/cpm-high-speed-steel-test-data\/","title":{"rendered":"CPM \uace0\uc18d\ub3c4\uac15 \uc2dc\ud5d8 \ub370\uc774\ud130, \ud15c\ud37c\ub9c1 \uc800\ud56d\uc131, \uace0\uc628 \uacbd\ub3c4 \ubc0f \uacf5\uad6c \uc218\uba85"},"content":{"rendered":"<h1 class=\"wp-block-heading\">CPM \uace0\uc18d\ub3c4\uac15 \uc2dc\ud5d8 \ub370\uc774\ud130, \ud15c\ud37c\ub9c1 \uc800\ud56d\uc131, \uace0\uc628 \uacbd\ub3c4 \ubc0f \uacf5\uad6c \uc218\uba85<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">P\/M \uace0\uc18d\ub3c4\uac15\uc740 \uace0\uc628\uacfc \uc808\uc0ad \ub0a0\uc5d0\uc11c\uc758 \uc131\ub2a5\uc744 \uc704\ud574 \uad6c\ub9e4\ub418\ubbc0\ub85c, \uc911\uc694\ud55c \uc218\uce58\ub294 \uc0c1\uc628 \uacbd\ub3c4 \uac12\uc774 \uc544\ub2d9\ub2c8\ub2e4. \uc774 \ud398\uc774\uc9c0\uc758 \ub124 \uac1c \ud45c\ub294 P\/M \uace0\uc18d\ub3c4\uac15 \ub4f1\uae09\uc744 \ub4b7\ubc1b\uce68\ud558\ub294 \uc2e4\ud5d8\uc2e4 \ub370\uc774\ud130\uc785\ub2c8\ub2e4: 595 \ubc0f 650 &#176;C\uc5d0\uc11c \uc7ac\ud15c\ud37c\ub9c1 \ud6c4 \uacbd\ub3c4\uac00 \uc5bc\ub9c8\ub098 \uc720\uc9c0\ub418\ub294\uc9c0, \uacf5\uad6c\uac00 \ub728\uac70\uc6b8 \ub54c \ub3d9\uc77c \uc628\ub3c4\uc5d0\uc11c \uacbd\ub3c4\uac00 \uc5bc\ub9c8\ub098 \ub0a8\ub294\uc9c0, 67.5 HRC\uc5d0\uc11c\uc758 \ucda9\uaca9 \uc5d0\ub108\uc9c0\uc640 \uad7d\ud798 \ud30c\ub2e8 \uac15\ub3c4, \uadf8\ub9ac\uace0 H13 \ub2e4\uc774\uac15 \ubc0f \ub2c8\ucf08 \ucd08\ud569\uae08\uc5d0 \ub300\ud55c CPM Rex 20 \ubc0f CPM Rex M42\uc758 \uc120\ubc18 \uacf5\uad6c \uc218\uba85\uc785\ub2c8\ub2e4. \ubaa8\ub4e0 \uac12\uc740 \uc6d0\ubb38 \uae30\uc0ac\uc5d0\uc11c \uc804\uccb4 \ud574\uc0c1\ub3c4\ub85c \uc77d\uc740 \uac83\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub124 \uac00\uc9c0 \uc2dc\ud5d8\uc774 \uce21\uc815\ud558\ub294 \uac83<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud15c\ud37c\ub9c1 \uc800\ud56d\uc131\uacfc \uace0\uc628 \uacbd\ub3c4\ub294 \uc11c\ub85c \ub2e4\ub978 \uc9c8\ubb38\uc5d0 \ub2f5\ud558\uba70 \ud45c\ub97c \ud63c\ub3d9\ud558\uae30 \uc27d\uc2b5\ub2c8\ub2e4. \ud15c\ud37c\ub9c1 \uc800\ud56d\uc131\uc740 \uac15\uc744 \uace0\uc628\uc5d0\uc11c \uc720\uc9c0\ud558\uace0 \ub0c9\uac01\ud55c \ud6c4 \uc0c1\uc628\uc5d0\uc11c \uce21\uc815\ud558\ubbc0\ub85c, \uacf5\uad6c\uac00 \uae30\uacc4\ub85c \ub3cc\uc544\uac14\uc744 \ub54c \uc5b4\ub5a4 \uc0c1\ud0dc\uc778\uc9c0 \uc54c\ub824\uc90d\ub2c8\ub2e4. \uace0\uc628 \uacbd\ub3c4\ub294 \uc2dc\ud3b8\uc774 \uc544\uc9c1 \ub728\uac70\uc6b4 \uc0c1\ud0dc\uc5d0\uc11c \uce21\uc815\ud558\ubbc0\ub85c, \uc808\uc0ad \uc911 \uc808\uc0ad \ub0a0\uc5d0\uc11c \uc5b4\ub5a4 \uc77c\uc774 \uc77c\uc5b4\ub098\ub294\uc9c0 \uc54c\ub824\uc90d\ub2c8\ub2e4. \ucda9\uaca9 \uc5d0\ub108\uc9c0\uc640 \uad7d\ud798 \ud30c\ub2e8 \uac15\ub3c4\ub294 \ub0a0\uc774 \uce58\ud551\ub420\uc9c0 \uc5ec\ubd80\ub97c \uc54c\ub824\uc8fc\uace0, \uc120\ubc18 \uc2dc\ud5d8\uc740 \uc774 \ubaa8\ub4e0 \uac83\uc774 \uacf5\uad6c \uc218\uba85 \ubd84\uc73c\ub85c \uc885\ud569\ud588\uc744 \ub54c \uc5b4\ub5a4 \uacb0\uacfc\uac00 \ub418\ub294\uc9c0 \uc54c\ub824\uc90d\ub2c8\ub2e4. \uace0\uc18d\ub3c4\uac15\uc740 \uac00\uaca9\uc5d0 \uac78\ub9de\uc73c\ub824\uba74 \ub124 \uac00\uc9c0 \ubaa8\ub450\ub97c \uacac\ub38c\uc57c \ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ubaa8\ub4e0 \ud45c\uc758 \uae30\uc900 \uc870\uac74\uc740 \ub3d9\uc77c\ud569\ub2c8\ub2e4. \ud569\uae08\uc740 1190 &#176;C (2175 &#176;F)\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ud558\uace0 550 &#176;C (1025 &#176;F)\uc5d0\uc11c 2\uc2dc\uac04\uc529 3\ud68c \ud15c\ud37c\ub9c1\ud588\uc73c\uba70, \uc774\ub294 \uad8c\uc7a5 \uacbd\ub3c4 \uc218\uce58\uac00 \uc778\uc6a9\ub418\ub294 \uae30\uc900 \ucc98\ub9ac\uc785\ub2c8\ub2e4. \uc7ac\ud15c\ud37c\ub9c1 \uc5f4\uc740 \uadf8\ub7f0 \ub2e4\uc74c \uac15\uc744 595 \ub610\ub294 650 &#176;C\uc5d0\uc11c \uc720\uc9c0\ud558\uace0 \uacbd\ub3c4\ub97c \ub2e4\uc2dc \uce21\uc815\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud15c\ud37c\ub9c1 \uc800\ud56d\uc131, \uace0\uc628 \ub178\ucd9c \ud6c4 \uacbd\ub3c4<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">550 &#176;C \uc5f4\uc740 \uae30\uc900\uc774\uba70 \uc138 \ud569\uae08 \ubaa8\ub450 67.5 HRC\uc5d0\uc11c \uc2dc\uc791\ud569\ub2c8\ub2e4. \uae30\uc874 M42\uc640 CPM Rex M42\ub294 \ub3d9\uc77c\ud55c \ud569\uae08\uc774\ubbc0\ub85c, \uc774\ub4e4 \uac04\uc758 \ube44\uad50\uac00 \uc774 \ud45c\uc758 \ud575\uc2ec\uc785\ub2c8\ub2e4. 595 &#176;C\uc5d0\uc11c 2\uc2dc\uac04\uc529 1\ud68c \ub610\ub294 2\ud68c \ud6c4, P\/M \uac15\uc740 65.5 \ubc0f 65 HRC\ub97c \uc720\uc9c0\ud558\ub294 \ubc18\uba74 \uae30\uc874 \uc81c\ud488\uc740 65 \ubc0f 65\ub85c, \ucc28\uc774\uac00 \uc791\uc544 \ub3d9\ub4f1\ud558\ub2e4\uace0 \ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. 650 &#176;C\uc5d0\uc11c\ub294 \ub458\uc774 \uac08\ub77c\uc9d1\ub2c8\ub2e4. CPM Rex M42\ub294 55.5 HRC\ub85c \ub05d\ub098\ub294 \ubc18\uba74 \uae30\uc874 M42\ub294 55\uc774\uba70, \ub2e4\ub974\uace0 \ub354 \ub9ce\uc774 \ud569\uae08\ub41c \ub4f1\uae09\uc778 CPM Rex 20\uc740 57 HRC\ub97c \uc720\uc9c0\ud569\ub2c8\ub2e4. \uc2e4\uc6a9\uc801\uc778 \ud574\uc11d\uc740 \ubd84\ub9d0 \uacf5\uc815 \uc790\uccb4\uac00 \ud15c\ud37c\ub9c1 \uc800\ud56d\uc131\uc744 \uc0ac\uc8fc\uc9c0\ub294 \uc54a\ub294\ub2e4\ub294 \uac83\uc785\ub2c8\ub2e4. \uc774\ub294 \ud569\uae08\uc758 \uae30\ub2a5\uc774\uba70, \ud145\uc2a4\ud150\uacfc \ucf54\ubc1c\ud2b8\uac00 \ub354 \ub9ce\uc774 \ud568\uc720\ub41c \ub4f1\uae09\uc740 \uc81c\uc870 \ubc29\uc2dd\uacfc \ubb34\uad00\ud558\uac8c \uace0\uc628\uc5d0\uc11c \ub354 \ub2e8\ub2e8\ud558\uac8c \uc720\uc9c0\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 3. CPM \ud569\uae08\uc758 \ud15c\ud37c\ub9c1 \uc800\ud56d\uc131, \ud45c\uc2dc\ub41c \ub178\ucd9c \ud6c4 HRC \uacbd\ub3c4<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud569\uae08 \ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">+550 &#176;C (1025 &#176;F) 3\ud68c\/2 h<\/th><th class=\"has-text-align-left\" data-align=\"left\">+595 &#176;C (1100 &#176;F)\/2 h<\/th><th class=\"has-text-align-left\" data-align=\"left\">+595 &#176;C (1100 &#176;F)\/2 + 2 h<\/th><th class=\"has-text-align-left\" data-align=\"left\">+650 &#176;C (1200 &#176;F)\/2 h<\/th><th class=\"has-text-align-left\" data-align=\"left\">+650 &#176;C (1200 &#176;F)\/2 + 2 h<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM Rex 20<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">66<\/td><td class=\"has-text-align-left\" data-align=\"left\">65.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">57<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM Rex M42<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">65.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">59<\/td><td class=\"has-text-align-left\" data-align=\"left\">55.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uae30\uc874 M42<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">59<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98: ASM Handbook Vol.1, P\/M Tool Steels \ud56d\ubaa9, Table 3. \uccab \ubc88\uc9f8 \uc5f4\uc740 \uae30\uc900 \uc0c1\ud0dc\ub85c, 1190 &#176;C (2175 &#176;F)\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ud558\uace0 550 &#176;C (1025 &#176;F)\uc5d0\uc11c 2\uc2dc\uac04\uc529 3\ud68c \ud15c\ud37c\ub9c1\ud55c \uc870\uac74\uc785\ub2c8\ub2e4. \ub098\uba38\uc9c0 \uc5f4\uc740 \ud574\ub2f9 \uc0c1\ud0dc\uc5d0 \ucd94\uac00 \ud15c\ud37c\ub9c1\uc744 \uc801\uc6a9\ud55c \uacb0\uacfc\uc785\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uace0\uc628 \uacbd\ub3c4, \uace0\uc628\uc5d0\uc11c \uce21\uc815<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc5ec\uae30\uc11c\ub294 \uc138 \uac00\uc9c0\uac00 \uc544\ub2cc \ub450 \ub4f1\uae09\uc774 \ubcf4\uace0\ub418\uba70, \uc2dc\ud3b8\uc774 \ub728\uac70\uc6b4 \uc0c1\ud0dc\uc5d0\uc11c \uce21\uc815\ud558\ubbc0\ub85c \uc218\uce58\uac00 \uc704 \ud45c\ubcf4\ub2e4 \ub0ae\uc2b5\ub2c8\ub2e4. \ub450 \ud569\uae08 \ubaa8\ub450 \uc0c1\uc628\uacfc 540 &#176;C \uc0ac\uc774\uc5d0\uc11c \uc57d 10 HRC\ub97c \uc783\uace0, 595 &#176;C\uc5d0\uc11c \ub458 \ub2e4 \uc57d 56 HRC\uc785\ub2c8\ub2e4. \ub9c8\uc9c0\ub9c9 \uc5f4\uc740 \uc8fc\ubaa9\ud560 \ub9cc\ud55c \ud655\uc778\uc785\ub2c8\ub2e4. 650 &#176;C \ub178\ucd9c \ud6c4 \uc2dc\ud3b8\uc744 \uc0c1\uc628\uc5d0\uc11c \ub2e4\uc2dc \uce21\uc815\ud558\uba74 CPM Rex 20\uc740 64 HRC, CPM Rex M42\ub294 63 HRC\ub85c \ub3cc\uc544\uc624\ubbc0\ub85c, \uace0\uc628\uc5d0\uc11c \uc783\uc740 \uacbd\ub3c4\ub294 \ub0c9\uac01 \uc2dc \ub300\ubd80\ubd84 \ud68c\ubcf5\ub418\uace0 \uacf5\uad6c\uac00 \ub728\uac70\uc6b4 \uc808\uc0ad\uc73c\ub85c \uc601\uad6c\uc801\uc73c\ub85c \uc5f0\ud654\ub418\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 4. CPM \ud569\uae08\uc758 \uace0\uc628 \uacbd\ub3c4, HRC<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud569\uae08 \ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc2dc\ud5d8 \uc804 \uc0c1\uc628<\/th><th class=\"has-text-align-left\" data-align=\"left\">540 &#176;C (1000 &#176;F)\uc5d0\uc11c<\/th><th class=\"has-text-align-left\" data-align=\"left\">595 &#176;C (1100 &#176;F)\uc5d0\uc11c<\/th><th class=\"has-text-align-left\" data-align=\"left\">650 &#176;C (1200 &#176;F)\uc5d0\uc11c<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc2dc\ud5d8 \ud6c4 \uc0c1\uc628<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM Rex 20<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">47.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM Rex M42<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">48.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, ASM Handbook Vol.1, P\/M Tool Steels \ub17c\ubb38, Table 4. Table 3\uacfc \ub3d9\uc77c\ud55c \uae30\uc900 \uc5f4\ucc98\ub9ac.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ucda9\uaca9 \uc5d0\ub108\uc9c0 \ubc0f \uad7d\ud798 \ud30c\ub2e8 \uac15\ub3c4<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \ud45c\ub294 \uacbd\ub3c4\ub97c 67.5 HRC\ub85c \uc77c\uc815\ud558\uac8c \uc720\uc9c0\ud558\uc5ec \ube44\uad50\uac00 \ub450 \uac00\uc9c0 \ub2e4\ub978 \ud15c\ud37c\ub9c1\uc774 \uc544\ub2cc \uc7ac\ub8cc \uac04\uc758 \ube44\uad50\uac00 \ub418\ub3c4\ub85d \ud588\uc73c\uba70, \uae30\uc0ac\uc5d0\uc11c \uac00\uc7a5 \uba85\ud655\ud55c \ub2e8\uc77c \uacb0\uacfc\uc785\ub2c8\ub2e4. CPM Rex 20\uacfc CPM Rex M42\ub294 \ub458 \ub2e4 \uc0e4\ub974\ud53c C-\ub178\uce58 \ucda9\uaca9 \uc5d0\ub108\uc9c0 16 J\uc744 \ud761\uc218\ud558\uace0 \uad7d\ud798 \ud30c\ub2e8 \uc2dc\ud5d8\uc5d0\uc11c \ub458 \ub2e4 4006 MPa (581 ksi)\uc5d0 \ub3c4\ub2ec\ud569\ub2c8\ub2e4. \ub3d9\uc77c \uacbd\ub3c4\uc758 \uae30\uc874 M42\ub294 7 J \ubc0f 2565 MPa (372 ksi)\ub97c \ud761\uc218\ud569\ub2c8\ub2e4. \ub3d9\uc77c \ud569\uae08\uc5d0\uc11c \ub3d9\uc77c \uacbd\ub3c4\ub85c \ucda9\uaca9 \uc5d0\ub108\uc9c0\ub294 \ub450 \ubc30 \uc774\uc0c1, \uad7d\ud798 \uac15\ub3c4\ub294 \uc57d 1.6\ubc30 \ub192\uc73c\uba70, CPM Rex M42\uc640 \uae30\uc874 M42\uc758 \uc720\uc77c\ud55c \ucc28\uc774\ub294 \uac15\uc774 \uc0dd\uc0b0\ub41c \ubc29\uc2dd\uc785\ub2c8\ub2e4. \uc774\uac83\uc774 \uc808\uc0ad \uacf5\uad6c\uc5d0\uc11c \ubd84\ub9d0 \uacf5\uc815\uc774 \ubc14\uafb8\ub294 \uac83\uc744 \uac00\uc7a5 \uba85\ud655\ud558\uac8c \ubcf4\uc5ec\uc8fc\ub294 \uc9c4\uc220\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 5. \ub450 CPM \ud569\uae08\uacfc \ud55c \uae30\uc874 \ud569\uae08\uc758 \uc0e4\ub974\ud53c C-\ub178\uce58 \ucda9\uaca9 \ubc0f \uad7d\ud798 \ud30c\ub2e8 \uac15\ub3c4<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud569\uae08 \ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654, &#176;C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654, &#176;F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4, HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc0e4\ub974\ud53c C-\ub178\uce58, J<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc0e4\ub974\ud53c C-\ub178\uce58, ft&#183;lbf<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uad7d\ud798 \ud30c\ub2e8 \uac15\ub3c4, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uad7d\ud798 \ud30c\ub2e8 \uac15\ub3c4, ksi<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM Rex 20<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">4006<\/td><td class=\"has-text-align-left\" data-align=\"left\">581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM Rex M42<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">4006<\/td><td class=\"has-text-align-left\" data-align=\"left\">581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uae30\uc874 M42<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2565<\/td><td class=\"has-text-align-left\" data-align=\"left\">372<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98: ASM Handbook Vol.1, P\/M Tool Steels \ud56d\ubaa9, Table 5. (a) \uc5fc\uc695\uc5d0\uc11c 4\ubd84 \uc720\uc9c0 \ud6c4 \uc720\ub0c9\ud558\uace0, 550 &#176;C (1025 &#176;F)\uc5d0\uc11c 2\uc2dc\uac04\uc529 3\ud68c \ud15c\ud37c\ub9c1.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">H13 \ubc0f \ub2c8\ucf08 \ucd08\ud569\uae08\uc5d0\uc11c\uc758 \uc120\ubc18 \uacf5\uad6c \uc218\uba85<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ub9c8\uc9c0\ub9c9 \ud45c\ub294 \uc704\uc758 \ubaa8\ub4e0 \uac83\uc744 \ubd84\uc73c\ub85c \ud658\uc0b0\ud569\ub2c8\ub2e4. \ub450 CPM \ub4f1\uae09\uc744 \ub2e8\uc77c \ud3ec\uc778\ud2b8 \uc120\uc0ad \uacf5\uad6c\ub85c 0.38 mm (0.015 in.)\uc758 \ud50c\ub7ad\ud06c \ub9c8\ubaa8\uac00 \ubc1c\uc0dd\ud560 \ub54c\uae4c\uc9c0 33 HRC\uc758 H13 \ub2e4\uc774\uac15 \ubc0f \ub2c8\ucf08 \uae30\ubc18 \ucd08\ud569\uae08\uc778 P\/M Ren&#233; 95\uc5d0 \ub300\ud574 \uc2e4\ud589\ud588\uc2b5\ub2c8\ub2e4. CPM Rex M42\ub294 H13\uc5d0\uc11c \ub2e8\uc18d \uc808\uc0ad \uc2dc 8\ubd84, \uc5f0\uc18d \uc808\uc0ad \uc2dc 16\ubd84 \uc9c0\uc18d\ub418\uc5c8\uace0, CPM Rex 20\uc740 8.5\ubd84 \ubc0f 14\ubd84 \uc9c0\uc18d\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \ucd08\ud569\uae08\uc5d0 \ub300\ud574\uc11c\ub294 \uc5f0\uc18d \uc808\uc0ad\uc774 0.20 m\/s (40 sfm) \ub300\uc2e0 0.06 m\/s (12 sfm)\ub85c \uc2e4\ud589\ub418\uc5c8\uace0 \uacf5\uad6c \uc218\uba85\uc740 \uae09\uaca9\ud788 \uc99d\uac00\ud558\uc5ec CPM Rex 20\uc740 31\ubd84, CPM Rex M42\ub294 27\ubd84\uc774\uc5c8\uc2b5\ub2c8\ub2e4. \uc138 \uc5f4\uc744 \uc544\ub798\uc758 \uc2dc\ud5d8 \uc870\uac74\uacfc \ud568\uaed8 \uc77d\uc73c\uc2ed\uc2dc\uc624. \uc18d\ub3c4\uac00 \ub3d9\uc77c\ud558\uc9c0 \uc54a\uc73c\uba70 \uc218\uce58\ub294 \uc5f4 \ub0b4\uc5d0\uc11c\ub9cc \ube44\uad50\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ud45c 6. CPM \ud569\uae08\uc758 \uc120\ubc18 \uacf5\uad6c \uc2dc\ud5d8 \uacb0\uacfc, 0.38 mm (0.015 in.) \ud50c\ub7ad\ud06c \ub9c8\ubaa8\uae4c\uc9c0\uc758 \uacf5\uad6c \uc218\uba85(\ubd84)<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud569\uae08 \ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654, &#176;C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654, &#176;F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4, HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">H13\uc5d0\uc11c\uc758 \ub2e8\uc18d \uc808\uc0ad, \ubd84<\/th><th class=\"has-text-align-left\" data-align=\"left\">H13 \uc5f0\uc18d \uc808\uc0ad, \ubd84<\/th><th class=\"has-text-align-left\" data-align=\"left\">P\/M Ren&#233; 95 \uc5f0\uc18d \uc808\uc0ad, \ubd84<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM Rex 20<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175<\/td><td class=\"has-text-align-left\" data-align=\"left\">67.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">31<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM Rex M42<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175<\/td><td class=\"has-text-align-left\" data-align=\"left\">67<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">27<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, ASM Handbook Vol.1, P\/M Tool Steels \ub17c\ubb38, Table 6.<\/em><\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Table 6\uc758 \uc2dc\ud5d8 \uc870\uac74<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc2dc\ud5d8 \uc870\uac74<\/th><th class=\"has-text-align-left\" data-align=\"left\">H13 \uac04\ud5d0 \uc808\uc0ad<\/th><th class=\"has-text-align-left\" data-align=\"left\">H13 \uc5f0\uc18d \uc808\uc0ad<\/th><th class=\"has-text-align-left\" data-align=\"left\">P\/M Ren&#233; 95 \uc5f0\uc18d \uc808\uc0ad<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc18d\ub3c4, m\/s (sfm)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20 (40)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20 (40)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06 (12)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc774\uc1a1, mm\/rev (in.\/rev)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.10 (0.004)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.14 (0.0055)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18 (0.007)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc808\uc0ad \uae4a\uc774, mm (in.)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.57 (0.062)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.57 (0.062)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.57 (0.062)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub0c9\uac01\uc218<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5c6\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5c6\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5c6\uc74c<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, ASM Handbook Vol.1, P\/M Tool Steels \ub17c\ubb38, Table 6 \uc2dc\ud5d8 \uc870\uac74 \ube14\ub85d.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub124 \uac1c\uc758 \ud45c\uac00 \ud568\uaed8 \ub9d0\ud558\ub294 \uac83<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud398\uc774\uc9c0 \uc804\uccb4\uc758 \ud328\ud134\uc740 \uc77c\uad00\ub418\uba70 \uad6c\ub9e4 \uacb0\uc815\uc744 \uc704\ud574 \uba85\ud655\ud788 \ubc1d\ud790 \uac00\uce58\uac00 \uc788\ub2e4. \ubd84\ub9d0 \uc57c\uae08 \uacbd\ub85c\ub294 \uc8fc\uc5b4\uc9c4 \uacbd\ub3c4\uc5d0\uc11c \uc778\uc131\uacfc \ub0a0\ub05d \uc548\uc804\uc131\uc744 \ud655\ubcf4\ud558\ub294\ub370, \uc774\ub294 Table 5\uac00 \ubcf4\uc5ec\uc8fc\ub294 \uac83\uc774\uace0 Table 6\uc774 \ubd84 \ub2e8\uc704\ub85c \uce21\uc815\ud558\ub294 \uac83\uc774\uba70, \uadf8 \uc790\uccb4\ub85c \uace0\uc628 \uacbd\ub3c4\ub098 \ud15c\ud37c\ub9c1 \uc800\ud56d\uc131\uc744 \ud655\ubcf4\ud558\uc9c0\ub294 \uc54a\ub294\ub370 \uc774\ub294 \uc131\ubd84\uacc4\uc5d0 \uc758\ud574 \uacb0\uc815\ub41c\ub2e4. \uae30\uc874 M42\ub098 T15\uc5d0\uc11c \ub0a0\ub05d\uc774 \ud30c\uc190\ub418\uac70\ub098 \uc774\ube68\uc774 \uce58\ud551\ub418\ub294 \ud604\uc7a5\uc774\ub77c\uba74 \ub3d9\uc77c \uba85\uce6d\uc758 P\/M \uac15\uc885\uc73c\ub85c \uc2e4\uc9c8\uc801\uc778 \uac1c\uc120\uc744 \uc5bb\uc744 \uc218 \uc788\ub2e4. \uc808\uc0ad \uc628\ub3c4\uc5d0\uc11c \uacf5\uad6c\uac00 \uc5f0\ud654\ub418\ub294 \uac83\uc774 \ubb38\uc81c\uc778 \ud604\uc7a5\uc774\ub77c\uba74 \uc774\ubbf8 \ubcf4\uc720\ud55c \uac15\uc885\uc758 P\/M \ubc84\uc804\uc774 \uc544\ub2c8\ub77c \ub354 \ub192\uac8c \ud569\uae08\ub41c \uac15\uc885\uc774 \ud544\uc694\ud558\uba70, \ucf54\ubc1c\ud2b8\uac00 \uadf8 \uc218\uce58\ub97c \uc6c0\uc9c1\uc774\ub294 \uc6d0\uc18c\uc774\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub2e4\uc74c\uc73c\ub85c \ubcfc \uacf3<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">CPM, ASP \ubc0f HAP \uac15\uc885\uc758 \uc870\uc131\uc740 <a href=\"https:\/\/aobosteel.com\/ko\/pm-tool-steel-composition-chart\/\">P\/M \uacf5\uad6c\uac15 \uc870\uc131 \ucc28\ud2b8<\/a>\uc5d0 \uc788\uc73c\uba70, \ub3d9\uc77c \uacc4\uc5f4\uc758 \ud0c4\ud654\ubb3c \ud06c\uae30, \ub0b4\ub9c8\ubaa8\uc131 \ubc0f \uc5f0\uc0ad\uc131 \ub370\uc774\ud130\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/pm-tool-steel-properties\/\">P\/M \uacf5\uad6c\uac15 \ud2b9\uc131 \ud398\uc774\uc9c0<\/a>\uc5d0 \uc788\ub2e4. \uae30\uc874 \uacf5\uad6c\uac15 \uacc4\uc5f4\uc758 \uace0\uc628 \uacbd\ub3c4\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-hot-hardness-chart\/\">\uacf5\uad6c\uac15 \uace0\uc628 \uacbd\ub3c4 \ucc28\ud2b8<\/a>\uc5d0 \uc815\ub9ac\ub418\uc5b4 \uc788\uc73c\uba70, \ud574\ub2f9 \uac15\uc885\uc758 \ucd5c\uc801 \ud15c\ud37c\ub9c1 \uc0c1\ud0dc\uc5d0\uc11c\uc758 \ucda9\uaca9 \uc5d0\ub108\uc9c0\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-impact-toughness-chart\/\">\uacf5\uad6c\uac15 \ucda9\uaca9 \uc778\uc131 \ucc28\ud2b8<\/a>\uc5d0 \uc788\ub2e4. Aobo Steel\uc740 \uae30\uc874 \uace0\uc18d\ub3c4\uac15\uc744 \ub2e8\uc870 \ubc0f \uc5f4\uac04 \uc555\uc5f0 \ubd09\uc7ac\ub85c \uacf5\uae09\ud558\uba70 \ub3c4\uba74\uc5d0 \ub530\ub77c P\/M \uacbd\ub85c\ub97c \uacac\uc801\ud560 \uc218 \uc788\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Vol 1, Properties and Selection: Irons, Steels and High-Performance Alloys.<\/p>","protected":false},"excerpt":{"rendered":"<p>CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life A P\/M high speed steel is bought for what it does at temperature and at the cutting edge, so the numbers that matter are not the room temperature hardness figures. The four tables on this page are the laboratory data behind the [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20812","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>CPM High Speed Steel, Temper Resistance and Tool Life<\/title>\n<meta name=\"description\" content=\"Temper resistance, hot hardness, impact energy, bend strength and lathe tool life data for the CPM high speed steel grades against conventional M42.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/cpm-high-speed-steel-test-data\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life\" \/>\n<meta property=\"og:description\" content=\"Temper resistance, hot hardness, impact energy, bend strength and lathe tool life data for the CPM high speed steel grades against conventional M42.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/cpm-high-speed-steel-test-data\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T17:16:22+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"7\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cpm-high-speed-steel-test-data\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cpm-high-speed-steel-test-data\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life\",\"datePublished\":\"2026-10-03T08:30:48+00:00\",\"dateModified\":\"2026-10-15T17:16:22+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cpm-high-speed-steel-test-data\\\/\"},\"wordCount\":1388,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cpm-high-speed-steel-test-data\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/cpm-high-speed-steel-test-data\\\/\",\"name\":\"CPM High Speed Steel, Temper Resistance and Tool Life\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-03T08:30:48+00:00\",\"dateModified\":\"2026-10-15T17:16:22+00:00\",\"description\":\"Temper resistance, hot hardness, impact energy, bend strength and lathe tool life data for the CPM high speed steel grades against conventional M42.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cpm-high-speed-steel-test-data\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/cpm-high-speed-steel-test-data\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cpm-high-speed-steel-test-data\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"CPM \uace0\uc18d\ub3c4\uac15, \ub0b4\ud15c\ud37c\ub9c1\uc131 \ubc0f \uacf5\uad6c \uc218\uba85","description":"CPM \uace0\uc18d\ub3c4 \uacf5\uad6c\uac15 \ub4f1\uae09\uacfc \uae30\uc874 M42\ub97c \ube44\uad50\ud55c \ud15c\ud37c\ub9c1 \uc800\ud56d\uc131, \uace0\uc628 \uacbd\ub3c4, \ucda9\uaca9 \uc5d0\ub108\uc9c0, \uad7d\ud798 \uac15\ub3c4 \ubc0f \uc120\ubc18 \uacf5\uad6c \uc218\uba85 \ub370\uc774\ud130\uc785\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/cpm-high-speed-steel-test-data\/","og_locale":"ko_KR","og_type":"article","og_title":"CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life","og_description":"Temper resistance, hot hardness, impact energy, bend strength and lathe tool life data for the CPM high speed steel grades against conventional M42.","og_url":"https:\/\/aobosteel.com\/ko\/cpm-high-speed-steel-test-data\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T17:16:22+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"7\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/cpm-high-speed-steel-test-data\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/cpm-high-speed-steel-test-data\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life","datePublished":"2026-10-03T08:30:48+00:00","dateModified":"2026-10-15T17:16:22+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/cpm-high-speed-steel-test-data\/"},"wordCount":1388,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/cpm-high-speed-steel-test-data\/","url":"https:\/\/aobosteel.com\/cpm-high-speed-steel-test-data\/","name":"CPM \uace0\uc18d\ub3c4\uac15, \ub0b4\ud15c\ud37c\ub9c1\uc131 \ubc0f \uacf5\uad6c \uc218\uba85","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-03T08:30:48+00:00","dateModified":"2026-10-15T17:16:22+00:00","description":"CPM \uace0\uc18d\ub3c4 \uacf5\uad6c\uac15 \ub4f1\uae09\uacfc \uae30\uc874 M42\ub97c \ube44\uad50\ud55c \ud15c\ud37c\ub9c1 \uc800\ud56d\uc131, \uace0\uc628 \uacbd\ub3c4, \ucda9\uaca9 \uc5d0\ub108\uc9c0, \uad7d\ud798 \uac15\ub3c4 \ubc0f \uc120\ubc18 \uacf5\uad6c \uc218\uba85 \ub370\uc774\ud130\uc785\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/cpm-high-speed-steel-test-data\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/cpm-high-speed-steel-test-data\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/cpm-high-speed-steel-test-data\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life A P\/M high speed steel is bought for what it does at temperature and at the cutting edge, so the numbers that matter are not the room temperature hardness figures. The four tables on this page are the laboratory data behind the&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"CPM High Speed Steel Test Data, Temper Resistance, Hot Hardness and Tool Life A P\/M high speed steel is bought for what it does at temperature and at the cutting edge, so the numbers that matter are not the room temperature hardness figures. The four tables on this page are the laboratory data behind the&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20812","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20812"}],"version-history":[{"count":3,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20812\/revisions"}],"predecessor-version":[{"id":22618,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20812\/revisions\/22618"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20812"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}