{"id":20624,"date":"2026-10-03T05:09:15","date_gmt":"2026-10-02T21:09:15","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20624"},"modified":"2026-10-16T00:58:14","modified_gmt":"2026-10-15T16:58:14","slug":"tool-steel-quenching-media-cooling-rates","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/tool-steel-quenching-media-cooling-rates\/","title":{"rendered":"\uacf5\uad6c\uac15\uc6a9 \ub2f4\uae08\uc9c8 \ub9e4\uccb4, \ub0c9\uac01 \uc18d\ub3c4 \ubc0f \ub2f4\uae08\uc9c8 \uac70\ub3d9"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\uacf5\uad6c\uac15\uc6a9 \ub2f4\uae08\uc9c8 \ub9e4\uccb4, \ub0c9\uac01 \uc18d\ub3c4 \ubc0f \ub2f4\uae08\uc9c8 \uac70\ub3d9<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\ub2f4\uae08\uc9c8\uc740 \ud558\ub098\uac00 \uc544\ub2cc \ub450 \uac1c\uc758 \uc218\uce58\ub85c \ud310\ub2e8\ub429\ub2c8\ub2e4. \uccab \ubc88\uc9f8\ub294 \ub9e4\uccb4\uac00 \ud384\ub77c\uc774\ud2b8\uc640 \ud0c4\ud654\ubb3c\uc774 \ud615\uc131\ub420 \uc218 \uc788\ub294 \ubc94\uc704\uc5d0\uc11c \ubd80\ud488\uc73c\ub85c\ubd80\ud130 \uc5f4\uc744 \uc5bc\ub9c8\ub098 \ube60\ub974\uac8c \ube7c\ub0b4\ub294\uc9c0\uc774\uba70, \ub450 \ubc88\uc9f8\ub294 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8 \uc2dc\uc791\uc810 \uc774\ud558\uc5d0\uc11c \uc5bc\ub9c8\ub098 \ube60\ub974\uac8c \ub0c9\uac01\uc744 \uc720\uc9c0\ud558\ub294\uc9c0\uc785\ub2c8\ub2e4. \uc5ec\uae30\uc11c \ucd94\uac00 \uc18d\ub3c4\ub294 \ubcc0\ud615\uacfc \uade0\uc5f4 \uc704\ud5d8\uc73c\ub85c \uc774\uc5b4\uc9d1\ub2c8\ub2e4. \uc544\ub798 \ud45c\ub294 \uc77c\ubc18\uc801\uc778 \ub2f4\uae08\uc9c8 \ub9e4\uccb4\uc758 \uacf5\uac1c\ub41c \ub0c9\uac01 \uc18d\ub3c4, \uc138 \uac00\uc9c0 \ub18d\ub3c4\uc5d0\uc11c \ud3f4\ub9ac\uba38 \ub2f4\uae08\uc9c8\uc81c\uc5d0 \ub300\ud574 \uce21\uc815\ub41c \uade0\uc5f4 \ubbfc\uac10\ub3c4\uc640 \ubcc0\ud615, \uadf8\ub9ac\uace0 \ub3d9\uc77c\ud55c \ub9e4\uccb4\uac00 \uc2dc\ud5d8\ubd09\uc758 \ub2e8\uba74\uc744 \ud1b5\ud574 \uc0dd\uc131\ud558\ub294 \uacbd\ub3c4\ub97c \uc218\uc9d1\ud55c \uac83\uc785\ub2c8\ub2e4. \ud568\uaed8 \uc77d\uc73c\uba74 \uc8fc\uc5b4\uc9c4 \ub2e8\uba74\uc744 \uc5b4\ub5a4 \ub9e4\uccb4\uc5d0\uc11c \ub2f4\uae08\uc9c8\ud560 \uc218 \uc788\ub294\uc9c0 \uc54c \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>\ucc38\uace0\uc6a9.<\/strong> \uc544\ub798 \uc218\uce58\ub294 \uacf5\uac1c\ub41c \uc911\uad6d \ud578\ub4dc\ubd81 \uad00\ud589\uc758 \ucc38\uace0 \uc694\uc57d\uc774\uba70, Aobo Steel\uc758 \uc0ac\uc591\uc774 \uc544\ub2d9\ub2c8\ub2e4. \uc8fc\ubb38\uc774\ub098 \uc0dd\uc0b0 \uc2e4\ud589\uc744 \uc774\uc5d0 \uadfc\uac70\ud558\uc5ec \uc124\uc815\ud558\uae30 \uc804\uc5d0 \ubc00 \uc778\uc99d\uc11c\uc640 \uad00\ub9ac \ub3c4\uba74\uc5d0 \ub300\ud574 \ub9e4\uccb4\uc640 \uc0ac\uc774\ud074\uc744 \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub2f4\uae08\uc9c8\uc774 \ud574\uc57c \ud558\ub294 \uc77c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uacbd\ud654\ub418\ub294 \ub2e8\uba74 \ub0b4\ubd80\uc5d0\uc11c \uac15\uc740 \ud384\ub77c\uc774\ud2b8\uc640 \ud0c4\ud654\ubb3c \ubc94\uc704\ub97c \ucda9\ubd84\ud788 \ube60\ub974\uac8c \ud1b5\uacfc\ud558\uc5ec \uadf8\ub7ec\ud55c \ubcc0\ud0dc\uac00 \uc2dc\uc791\ub418\uc9c0 \uc54a\uc544\uc57c \ud558\uba70, \uc2a4\uc2a4\ub85c \ud30c\uad34\ub418\uc9c0 \uc54a\uace0 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8 \ubc94\uc704\uc5d0 \ub3c4\ub2ec\ud574\uc57c \ud569\ub2c8\ub2e4. \ub108\ubb34 \ub290\ub9b0 \ub2f4\uae08\uc9c8\uc740 \ub450\uaebc\uc6b4 \ub2e8\uba74\uc5d0 \uc5f0\ud55c \ubd80\ubd84\uc744 \ub0a8\uae41\ub2c8\ub2e4. \uac15\uc885\uc774 \ud544\uc694\ub85c \ud558\ub294 \uac83\ubcf4\ub2e4 \ube60\ub978 \ub2f4\uae08\uc9c8\uc740 \uc544\ubb34 \uc774\uc720 \uc5c6\uc774 \ubcc0\ud615\uacfc \uade0\uc5f4 \uc704\ud5d8\uc744 \ucd94\uac00\ud569\ub2c8\ub2e4. \ub530\ub77c\uc11c \ub9e4\uccb4\uc758 \ub0c9\uac01 \uc18d\ub3c4\ub294 \ub2e8\uc77c \uc218\uce58\uac00 \uc544\ub2c8\ub77c \ub450 \uac1c\uc758 \ubcc4\ub3c4 \uc628\ub3c4 \ucc3d\uc5d0\uc11c \uc77d\ud788\uba70, \uc774 \ud398\uc774\uc9c0\uc758 \ubaa8\ub4e0 \ud45c\ub294 \uadf8\ub807\uac8c \uad6c\uc131\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. \uc0c1\ubd80 \ucc3d\uc778 650~500\u00b0C\ub294 \uc5f0\ud55c \ubd80\ubd84\uc758 \uc2b9\ud328\uac00 \uacb0\uc815\ub418\ub294 \uacf3\uc785\ub2c8\ub2e4. \ud558\ubd80 \ucc3d\uc778 300~200\u00b0C\ub294 \uade0\uc5f4\uacfc \ubcc0\ud615\uc758 \uc2b9\ud328\uac00 \uacb0\uc815\ub418\ub294 \uacf3\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ubd80\ud488\uc774 \ub0c9\uac01\ub418\ub294 \ub3d9\uc548 \ud1b5\uacfc\ud558\ub294 \uc138 \ub2e8\uacc4\ub294 \ub9e4\uccb4\uac00 \uc120\ud0dd\ub418\ub294 \uae30\uc900\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg\" alt=\"Mechanism of heat transfer during film boiling: the vapour blanket, the surface heat fluxes and the temperature and flow velocity in the boundary layer during immersion quenching\"\/><figcaption class=\"wp-element-caption\">\uadf8\ub9bc 9.27. \ub9c9\ube44\ub4f1 \ub3d9\uc548 \ud45c\uba74\uc5d0\uc11c\uc758 \uc5f4\uc804\ub2ec\ub85c, \uacbd\uacc4\uce35 \ub0b4 \uc628\ub3c4 \ubc0f \uc720\uc18d \ubd84\ud3ec\ub97c \ub098\ud0c0\ub0b8\ub2e4. \uc5f4\uc740 \uc804\ub3c4(q1)\uc640 \ubcf5\uc0ac(q2)\uc5d0 \uc758\ud574 \uc99d\uae30\ub9c9\uc744 \ud1b5\uacfc\ud558\uba70, \uc77c\ubd80 q3\ub9cc\uc774 \ub300\ub958\uc5d0 \uc758\ud574 \uc561\uccb4\uc5d0 \ub3c4\ub2ec\ud558\uace0, \ub098\uba38\uc9c0 q4\ub294 \ub2f4\uae08\uc9c8\uc81c\ub97c \uae30\ud654\uc2dc\ucf1c \uc99d\uae30\ub9c9\uc744 \uc720\uc9c0\ud55c\ub2e4. \uce68\uc801 \ub2f4\uae08\uc9c8 \uc18d\ub3c4 w\ub294 \ud45c\uba74 \uc544\ub798\uc5d0 \ud45c\uc2dc\ub418\uc5b4 \uc788\ub2e4. \uc774\uac83\uc774 \uc99d\uae30\ub9c9 \ub2e8\uacc4\uc774\uba70, \uc774 \ub2e8\uacc4\uc5d0\uc11c \uc99d\uae30\ub9c9\uc774 \ubd95\uad34\ub418\uae30 \uc804\uc5d0 \ub2e8\uba74\uc774 \ud384\ub77c\uc774\ud2b8 \ub178\uc988\ub97c \ud1b5\uacfc\ud558\ub294\uc9c0 \uc5ec\ubd80\uac00 \uacb0\uc815\ub41c\ub2e4. \ucd9c\ucc98: H.M. Tensi, A. Stich and G.E. Totten, Quenching and Quenching Technology, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 9.27.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">\uc77c\ubc18\uc801\uc778 \ub2f4\uae08\uc9c8 \ub9e4\uccb4\uc758 \ub0c9\uac01 \uc18d\ub3c4<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uccab \ubc88\uc9f8 \ud45c\uc758 \uc18d\ub3c4\ub294 20 mm \uac15\uad6c\uc5d0\uc11c \uce21\uc815\ub418\uc5c8\uc73c\uba70 \uac01 \ub9e4\uccb4\uc758 \uacf5\uac1c\ub41c \ub0c9\uac01 \uace1\uc120\uc5d0\uc11c \ucd94\uc815\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uccab \ubc88\uc9f8 \uc5f4\uc740 \ub9e4\uccb4\uac00 \uac00\uc7a5 \ube60\ub974\uac8c \ub0c9\uac01\ub418\ub294 \uc628\ub3c4\uc774\uace0, \ub450 \ubc88\uc9f8\ub294 \uadf8 \ucd5c\ub300 \uc18d\ub3c4\uc774\uba70, \ub9c8\uc9c0\ub9c9 \ub450 \uac1c\ub294 \uc0c1\ubd80 \ubc0f \ud558\ubd80 \ucc3d \uc804\uccb4\uc758 \ud3c9\uade0 \uc18d\ub3c4\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub9e4\uccb4\uac00 \ud574\ub2f9 \ub0c9\uac01 \uc18d\ub3c4\ub97c \uc804\ub2ec\ud558\ub294 \ubc29\uc2dd\uc740 \ubd80\ud488 \uc790\uccb4\uc5d0\uc11c \ud655\uc778\ud560 \uc218 \uc788\ub294\ub370, \uc774\ub294 \ube60\ub978 \ub0c9\uac01\uc774 \uc2dc\uc791\ub418\uae30 \uc804\uc5d0 \uc99d\uae30\ub9c9\uc774 \ud30c\uad34\ub418\uc5b4\uc57c \ud558\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-9-wetting-crni-cylinder-water-oil.jpg\" alt=\"Wetting of a 25 mm by 100 mm CrNi steel cylinder quenched from 850 C, photographed at fixed times in water and in oil\"\/><figcaption class=\"wp-element-caption\">\uadf8\ub9bc 9.9. 850 &#176;C\uc5d0\uc11c \ub2f4\uae08\uc9c8\ud55c CrNi \uac15 \uc2e4\ub9b0\ub354\uc758 \uc816\uc74c \uacfc\uc815\uc744 \uc77c\uc815 \uc2dc\uac04\ub9c8\ub2e4 \ucd2c\uc601\ud55c \uc0ac\uc9c4\uc785\ub2c8\ub2e4: (a) 30 &#176;C \ubb3c\uc5d0\uc11c 0.3 m\/s\ub85c \uc720\ub3d9\ud558\ub294 \uc870\uac74\uc758 25 mm &#215; 100 mm \uc2e4\ub9b0\ub354, (b) 60 &#176;C \uc624\uc77c\uc5d0\uc11c 0.3 m\/s\ub85c \uc720\ub3d9\ud558\ub294 \uc870\uac74\uc758 \ub3d9\uc77c \uc2e4\ub9b0\ub354, (c) \ubb3c \uc18d\uc758 15 &#215; 15 &#215; 45 mm \uac01\uae30\ub465 \uc2dc\ud3b8. \uc99d\uae30\ub9c9\uc740 \ubd80\ud488 \ud558\ub2e8\uc5d0\uc11c \ud30c\uad34\ub418\uace0 \uc816\uc740 \uc601\uc5ed\uc774 \ud45c\uba74\uc744 \ub530\ub77c \uc704\ub85c \uc774\ub3d9\ud558\ub294\ub370, \uc774\uac83\uc774 \ud558\ub2e8\uc758 \uad50\ubc18\uc774 \uc99d\uae30\ub9c9 \ub2e8\uacc4\ub97c \ub2e8\ucd95\uc2dc\ud0a4\ub294 \uc774\uc720\uc785\ub2c8\ub2e4. \uc608\uc2dc \uc18c\uc7ac\ub294 \uacf5\uad6c\uac15\uc774 \uc544\ub2cc \ud06c\ub86c-\ub2c8\ucf08 \uac15\uc774\uba70, \uacf5\uad6c\uac15\uc5d0\uc11c\ub3c4 \uc21c\uc11c\ub294 \uac19\uace0 \uc2dc\uac04\ub9cc \ub2e4\ub985\ub2c8\ub2e4. \ucd9c\ucc98: H.M. Tensi, A. Stich \ubc0f G.E. Totten, Quenching and Quenching Technology, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 9.9.<\/figcaption><\/figure>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \uc18d\ub3c4 \uc9c0\uc810, &deg;C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \uc18d\ub3c4, &deg;C\/s<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 650&ndash;500 &deg;C, &deg;C\/s<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 300&ndash;200 &deg;C, &deg;C\/s<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc815\uc9c0 \uc218\ub3d7\ubb3c, 20 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">340<\/td><td class=\"has-text-align-left\" data-align=\"left\">775<\/td><td class=\"has-text-align-left\" data-align=\"left\">135<\/td><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc815\uc9c0 \uc218\ub3d7\ubb3c, 40 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">285<\/td><td class=\"has-text-align-left\" data-align=\"left\">545<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">410<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc815\uc9c0 \uc218\ub3d7\ubb3c, 60 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">220<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">185<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% NaCl \uc6a9\uc561, 20 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">580<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">1900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">15% NaOH \uc6a9\uc561, 20 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">560<\/td><td class=\"has-text-align-left\" data-align=\"left\">2830<\/td><td class=\"has-text-align-left\" data-align=\"left\">2750<\/td><td class=\"has-text-align-left\" data-align=\"left\">775<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5% Na<sub>2<\/sub>CO<sub>3<\/sub> \uc6a9\uc561, 20 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">430<\/td><td class=\"has-text-align-left\" data-align=\"left\">1640<\/td><td class=\"has-text-align-left\" data-align=\"left\">1140<\/td><td class=\"has-text-align-left\" data-align=\"left\">820<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L-AN15 \uc21c\uc720, 20 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">430<\/td><td class=\"has-text-align-left\" data-align=\"left\">230<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L-AN15 \uc21c\uc720, 80 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">430<\/td><td class=\"has-text-align-left\" data-align=\"left\">230<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L-AN32 \uc21c\uc720, 20 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">500<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c 8-9, \uc778\uc1c4 \ud398\uc774\uc9c0 464. \ub0c9\uac01 \uc18d\ub3c4\ub294 20 mm \uac15\uad6c\uc5d0\uc11c \uce21\uc815\ub418\uc5c8\uc73c\uba70 \uac01 \ub9e4\uccb4\uc758 \ub0c9\uac01 \uace1\uc120\uc5d0\uc11c \ucd94\uc815\ub418\uc5c8\uc2b5\ub2c8\ub2e4. L-AN \ub4f1\uae09\uc740 \uc911\uad6d\uc2dd \uc804\uc190\uc2e4 \uc2dc\uc2a4\ud15c \uc624\uc77c\ub85c, L-AN15\ub294 ISO VG15\uc5d0 \uac00\uae5d\uace0 L-AN32\ub294 ISO VG32\uc5d0 \uac00\uae5d\uc2b5\ub2c8\ub2e4. \ubc31\ubd84\uc728\uc740 \uc9c8\ub7c9 \ubd84\uc728\uc785\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub3d9\uc77c\ud55c \uc0c1\uad00\uad00\uacc4\uac00 \ud45c\uc900 \uc11c\uc591\uc2dd \ub0c9\uac01 \uac15\ub3c4 \ucc99\ub3c4\uc5d0\ub3c4 \ub098\ud0c0\ub098\uba70, \uc774\ub294 \ub9e4\uccb4\uc640 \uad50\ubc18\uc774 \ud568\uaed8 \uc81c\uacf5\ud558\ub294 \uac83\uc744 \uc218\uce58\ub85c \ub098\ud0c0\ub0c5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-table-9-3-grossman-h-factor-heat-transfer-coefficient.jpg\" alt=\"Grossman H factor and the corresponding heat transfer coefficient for air, conventional oil, fast oil and water, at several bath temperatures and quenchant velocities\"\/><figcaption class=\"wp-element-caption\">\ud45c 9.3. \uc5ec\ub7ec \uc695\uc870 \uc628\ub3c4\uc640 \ub2f4\uae08\uc9c8\uc81c \uc720\uc18d \uc870\uac74\uc5d0\uc11c \uc120\ud0dd\ub41c \ub2f4\uae08\uc9c8\uc81c(\uacf5\uae30, \uc77c\ubc18 \uc624\uc77c, \uace0\uc18d \uc624\uc77c, \ubb3c)\uc5d0 \ub300\ud55c Grossman H \uacc4\uc218\uc640 \uadf8\uc5d0 \ub300\uc751\ud558\ub294 \uc5f4\uc804\ub2ec \uacc4\uc218\uc785\ub2c8\ub2e4. H \uac12\uc740 \uacbd\ud654\ub2a5 \uc120\ub3c4\uc640 \ud568\uaed8 \uc0ac\uc6a9\ud558\ub294 \ub2f4\uae08\uc9c8 \uac15\ub3c4 \uc9c0\uc218\uc774\ubbc0\ub85c, \uc774 \ud45c\ub294 \uac15\ub3c4 \uc911 \uc5bc\ub9c8\uac00 \ub9e4\uccb4\uc5d0\uc11c \uc624\uace0 \uc5bc\ub9c8\uac00 \uad50\ubc18\uc5d0\uc11c \uc624\ub294\uc9c0\ub97c \ubcf4\uc5ec \uc90d\ub2c8\ub2e4. 32 &#176;C\uc758 \ubb3c\uc740 \uc815\uc9c0 \uc0c1\ud0dc\uc758 H 1.1\uc5d0\uc11c 0.76 m\/s\uc5d0\uc11c H 2.8\uae4c\uc9c0 \uc62c\ub77c\uac11\ub2c8\ub2e4. \uc704\uc5d0\uc11c \uc124\uba85\ud55c \ub3d9\uc77c\ud55c \ub9e4\uccb4\uc5d0 \ub300\ud55c \ub450 \ubc88\uc9f8 \uad50\ucc28 \uac80\uc99d \ucc99\ub3c4\ub85c \uc77d\uc73c\uc2ed\uc2dc\uc624. \ucd9c\ucc98: H.M. Tensi, A. Stich \ubc0f G.E. Totten, Quenching and Quenching Technology, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Table 9.3.<\/figcaption><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ud328\ud134\uc740 \uacf5\uad6c \uc791\uc5c5\uc7a5\uc5d0\uc11c \ub2e4\ub8e8\ub294 \ubc29\uc2dd\uc785\ub2c8\ub2e4. \ubb3c\uc740 \ube60\ub974\uba70 \uc695\uc870\uac00 \ub530\ub73b\ud574\uc9c8\uc218\ub85d \ub290\ub824\uc9c0\ubbc0\ub85c \ub728\uac70\uc6b4 \ubb3c \uc695\uc870\ub294 \uc81c\uc5b4\ub41c \ub2f4\uae08\uc9c8\uc758 \ub300\uccb4\ubb3c\uc774 \uc544\ub2d9\ub2c8\ub2e4. 10% \uc18c\uae08\ubb3c \ub610\ub294 \uac00\uc131 \uc695\uc870\ub294 \uc0c1\ubd80 \ucc3d\uc5d0\uc11c \uc815\uc9c0 \ubb3c\ubcf4\ub2e4 \uc57d \uc138 \ubc30 \ube60\ub974\uba70, \uc774\ub294 \uc800\uacbd\ud654\ub2a5 \ud0c4\uc18c\uac15\uc758 \uc5f0\ud55c \ubd80\ubd84\uc744 \uc81c\uac70\ud558\ub294 \uc694\uc778\uc774\uba70, \ub458 \ub2e4 300\u00b0C \uc774\ud558\uc5d0\uc11c\ub3c4 \ube60\ub974\uac8c \uc720\uc9c0\ub418\ubbc0\ub85c \uc587\uc740 \ub2e8\uba74\uc744 \uade0\uc5f4\uc2dc\ud0a4\ub294 \uc774\uc720\uc785\ub2c8\ub2e4. \uc21c\uc720\ub294 \uc0c1\ubd80 \ucc3d\uc5d0\uc11c \ubb3c\ubcf4\ub2e4 \ud55c \uc790\ub9bf\uc218 \ub290\ub9ac\uace0 \ud558\ubd80 \ucc3d\uc5d0\uc11c\ub3c4 \ub9c8\ucc2c\uac00\uc9c0\ub85c \ub290\ub9ac\ubbc0\ub85c, \uc624\uc77c\uc774 \ud384\ub77c\uc774\ud2b8 \ubc94\uc704\ub97c \ub290\ub9ac\uac8c \ud1b5\uacfc\ud574\ub3c4 \uacac\ub51c \ub9cc\ud07c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uac00 \uc548\uc815\uc801\uc778 \uac15\uc885\uc5d0 \uc801\ud569\ud55c \uc774\uc720\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub2f4\uae08\uc9c8\uc774 \ubcc0\ud0dc \ubc94\uc704\ub97c \ud1b5\uacfc\ud560 \uc218 \uc788\ub294 \ub124 \uac00\uc9c0 \uacbd\ub85c\uac00 \uc544\ub798\uc5d0 \uc124\uba85\ub418\uc5b4 \uc788\ub294\ub370, \uc774\ub294 \ub9e4\uccb4\uac00 \uc120\ud0dd\ub418\ub294 \uc5ec\ub7ec \uc635\uc158 \uc911 \ud558\ub098\uc77c \ubfd0\uc774\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-8-cooling-curves-quenching-methods.jpg\" alt=\"Cooling curves for the centre and the surface of quenched parts for direct quenching, marquenching, austempering and isothermal annealing, correlated to a time-temperature transformation diagram\"\/><figcaption class=\"wp-element-caption\">\uadf8\ub9bc 9.8. \ub124 \uac00\uc9c0 \ub2f4\uae08\uc9c8 \uacbd\ub85c\uc5d0 \ub300\ud55c \ub2f4\uae08\uc9c8\ub41c \ubd80\ud488\uc758 \uc911\uc2ec\uacfc \ud45c\uba74\uc5d0\uc11c\uc758 \ub0c9\uac01 \uace1\uc120\uc744 \uc2dc\uac04-\uc628\ub3c4 \ubcc0\ud0dc \uc120\ub3c4\uc5d0 \ub300\ud574 \ub098\ud0c0\ub0b8 \uac83: (a) \uc9c1\uc811 \ub2f4\uae08\uc9c8, (b) \ub9c8\ub974\ud01c\uce6d, (c) \uc624\uc2a4\ud15c\ud37c\ub9c1, (d) \ub4f1\uc628 \uc5b4\ub2d0\ub9c1 \ub610\ub294 \ud384\ub77c\uc774\ud2b8\ud654. \uc9c1\uc811 \ub2f4\uae08\uc9c8\uc740 \uc804\uccb4 \ubcc0\ud0dc \ubc94\uc704\ub97c \ud55c \ubc88\uc5d0 \ud1b5\uacfc\ud558\uc5ec \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\ub97c \uc0dd\uc131\ud558\uace0, \ub9c8\ub974\ud01c\uce6d\uc740 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8 \uc2dc\uc791 \uc628\ub3c4 \uc704\uc5d0\uc11c \uc815\uc9c0\ud558\uc5ec \ub2e8\uba74\uc744 \uade0\uc77c\ud654\ud558\uace0 \uacf5\uae30 \uc911\uc5d0\uc11c \ubcc0\ud0dc\ub97c \uc644\ub8cc\ud558\uba70, \uc624\uc2a4\ud15c\ud37c\ub9c1\uc740 \ubca0\uc774\ub098\uc774\ud2b8 \ubc94\uc704\uc5d0\uc11c \uc720\uc9c0\ud558\uace0, \ub4f1\uc628 \uc5b4\ub2d0\ub9c1\uc740 \ud384\ub77c\uc774\ud2b8\ub97c \uc0dd\uc131\ud560 \ub9cc\ud07c \ucda9\ubd84\ud788 \ub192\uac8c \uc720\uc9c0\ud569\ub2c8\ub2e4. \uc608\uc2dc \uac15\uc740 \ud0c4\uc18c\uac15\uc774\uba70 \ub3d9\uc77c\ud55c \ub124 \uac00\uc9c0 \uacbd\ub85c\uac00 \uacf5\uad6c\uac15\uc5d0\ub3c4 \uc801\uc6a9\ub429\ub2c8\ub2e4. \ucd9c\ucc98: H.M. Tensi, A. Stich and G.E. Totten, Quenching and Quenching Technology, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 9.8.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">\ubb3c\uacfc \uc624\uc77c\uc5d0 \ub300\ud55c \uc18c\uae08 \ubc0f \uac00\uc131 \uc6a9\uc561<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud3ec\ud654 \uc5fc\ud654\uce7c\uc298 \uc6a9\uc561\uc740 \uc18c\uae08\ubb3c\uacfc \uc624\uc77c \uc0ac\uc774\uc5d0 \uc704\uce58\ud558\ub294 \ub9e4\uccb4\ub85c \uac1c\ubc1c\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uadf8 \uade0\uc5f4 \uac70\ub3d9\uc740 \uc624\uc77c\ubcf4\ub2e4 \ubb3c\uc5d0 \uac00\uae5d\uc9c0\ub9cc, \uc0c1\ubd80 \ucc3d\uc5d0\uc11c\uc758 \uc18d\ub3c4\ub294 \ud0c4\uc18c\uac15\uc5d0 \ucda9\ubd84\ud560 \ub9cc\ud07c \ub192\uc2b5\ub2c8\ub2e4. \ub450 \ubc88\uc9f8 \ud45c\ub294 \ub3d9\uc77c\ud55c \ub450 \ucc3d\uc5d0\uc11c \uce21\uc815\ub41c \ub2e4\ub978 \uc77c\ubc18 \ub9e4\uccb4\uc640 \ube44\uad50\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub450 \ub9e4\uccb4\uac00 \uc800\uc628 \uc601\uc5ed\uc5d0\uc11c \uc774\ub807\uac8c \ub2e4\ub974\uac8c \uac70\ub3d9\ud558\ub294 \uc774\uc720\ub294 \uc5f4\uc804\ub2ec \uacc4\uc218 \uace1\uc120\uc5d0 \uae30\ub85d\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-21-heat-transfer-coefficient-water-oil.jpg\" alt=\"Heat transfer coefficient against surface temperature of an austenitic steel cylinder quenched into water at 30 C and into a fast oil at 60 C, both flowing at 0.3 m\/s\"\/><figcaption class=\"wp-element-caption\">\uadf8\ub9bc 9.21. 25 mm &#215; 100 mm \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uacc4 \uac15 \uc2e4\ub9b0\ub354\ub97c 30 &#176;C \ubb3c\uacfc 60 &#176;C \uace0\uc18d \uc624\uc77c\uc5d0 \uac01\uac01 0.3 m\/s\ub85c \uc720\ub3d9\uc2dc\ud0a4\uba70 \ub2f4\uae08\uc9c8\ud588\uc744 \ub54c\uc758 \ud45c\uba74 \uc628\ub3c4\uc5d0 \ub300\ud55c \uc5f4\uc804\ub2ec \uacc4\uc218\uc785\ub2c8\ub2e4. \ubb3c \uace1\uc120\uc740 \uc57d 15,000 W\/(m&#178;K)\uc5d0\uc11c \ucd5c\ub300\uac12\uc744 \ubcf4\uc774\ub294\ub370, \uc774\ub294 \uc99d\uae30\ub9c9\uc774 \ubd95\uad34\ub41c \ud6c4\uc758 \ud575\ube44\ub4f1 \ud2b9\uc720\uc758 \ud615\ud0dc\uc785\ub2c8\ub2e4. \uc624\uc77c \uace1\uc120\uc740 \uac19\uc740 \uc628\ub3c4 \ubc94\uc704\uc5d0\uc11c \ud55c \uc790\ub9bf\uc218 \ub0ae\uace0 \ud6e8\uc52c \ud3c9\ud0c4\ud569\ub2c8\ub2e4. \uc774 \ud55c \uac00\uc9c0 \ucc28\uc774\uac00 \ubb3c\uc774 \ub450\uaebc\uc6b4 \ub2e8\uba74\uc744 \uacbd\ud654\uc2dc\ud0a4\uace0 \uc587\uc740 \ub2e8\uba74\uc744 \uade0\uc5f4\uc2dc\ud0a4\ub294 \uc774\uc720\uc774\uba70, \uc624\uc77c\uc774 \uadf8 \ubc18\ub300\uc778 \uc774\uc720\uc785\ub2c8\ub2e4. \ucd9c\ucc98: H.M. Tensi, A. Stich \ubc0f G.E. Totten, Quenching and Quenching Technology, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 9.21.<\/figcaption><\/figure>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 650&ndash;550 &deg;C, &deg;C\/s<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 300&ndash;200 &deg;C, &deg;C\/s<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud3ec\ud654 CaCl<sub>2<\/sub> \uc6a9\uc561<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubb3c, 18 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">270<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% NaCl \uc6a9\uc561, 20 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">15% NaOH \uc6a9\uc561, 20 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc720\ucc44\uc720, 50 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">200<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L-AN15 \uc21c\uc720, 50 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubcc0\uc555\uae30 \uc624\uc77c, 50 &deg;C<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c 8-10, \uc778\uc1c4 \ud398\uc774\uc9c0 465. \uac01 \ubc94\uc704\uc758 \ud3c9\uade0 \ub0c9\uac01 \uc18d\ub3c4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud3f4\ub9ac\uba38 \ub2f4\uae08\uc9c8\uc81c, \uade0\uc5f4 \ubc0f \ubcc0\ud615<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud3f4\ub9ac\uba38 \ub2f4\uae08\uc9c8\uc81c\ub294 \ub18d\ub3c4\uc5d0 \ub530\ub77c \ub0c9\uac01 \uc18d\ub3c4\uac00 \uacb0\uc815\ub418\ub294 \uc218\uc6a9\uc561\uc774\ubbc0\ub85c, \ud558\ub098\uc758 \uc695\uc870\uac00 \ud3f4\ub9ac\uba38 \ud568\ub7c9\uc744 \ubcc0\uacbd\ud558\uc5ec \uc18c\uae08\ubb3c\uc5d0\uc11c \uc624\uc77c\uae4c\uc9c0\uc758 \ubc94\uc704\ub97c \ucee4\ubc84\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc544\ub798 \uc138 \ud45c\ub294 \uc911\uad6d NQ-1 \ud3f4\ub9ac\uba38\uc5d0 \ub300\ud55c \ud558\ub098\uc758 \uc2dc\ud5d8 \ud504\ub85c\uadf8\ub7a8\uc5d0\uc11c \ub098\uc628 \uac83\uc73c\ub85c, \uc9c8\ub7c9 \uae30\uc900 5%, 15%, 25%\uc5d0\uc11c \ubb3c\uacfc \uc21c\uc720\ub97c \uae30\uc900 \ub9e4\uccb4\ub85c \uc0ac\uc6a9\ud558\uc5ec \uc2e4\ud589\ub418\uc5c8\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\uade0\uc5f4 \ubbfc\uac10\ub3c4<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\uade0\uc5f4 \uc2dc\ud5d8\uc740 30 mm x 30 mm T8 \ud0c4\uc18c \uacf5\uad6c\uac15 \uc2dc\ud3b8\uc744 \uc0ac\uc6a9\ud558\uc5ec 840\u00b0C\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ud558\uace0 30\ubd84\uac04 \uc720\uc9c0\ud55c \ud6c4 \ub2f4\uae08\uc9c8 \ud6c4 \uc790\uae30 \uc785\uc790 \uac80\uc0ac\ub85c \ud655\uc778\ud588\uc2b5\ub2c8\ub2e4. \uac01 \ub9e4\uccb4\uc5d0 \ub300\ud574 \uc138 \uac1c\uc758 \uc2dc\ud3b8\uc744 \uc2e4\ud589\ud588\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc2dc\ud3b8<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uade0\uc5f4 \ubc1c\uc0dd<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc218\ub0c9<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">15% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">25% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L-AN15 \uc21c\uc720<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c 8-11, \uc778\uc1c4 \ud398\uc774\uc9c0 466. T8 \ud0c4\uc18c \uacf5\uad6c\uac15, 30 mm \u00d7 30 mm, 840\u00b0C\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ud558\uace0 30\ubd84 \uc720\uc9c0, \uc790\ubd84\ud0d0\uc0c1\uac80\uc0ac\ub85c \ud655\uc778.<\/em><\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2e8\uba74 \uacbd\ub3c4<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\uacbd\ud654\ub2a5 \uc2dc\ud5d8\uc5d0\ub294 \ubcf4\ud1b5 \ud0c4\uc18c\uac15\uc778 45\uac15\uc744 \ub450 \uac00\uc9c0 \ubd09\uc7ac \ud06c\uae30\ub85c \uc0ac\uc6a9\ud588\uc2b5\ub2c8\ub2e4. \uacbd\ub3c4\ub294 \ucd95 \ubc29\ud5a5\uc73c\ub85c \uc808\ub2e8\ud55c \ubd09\uc7ac\uc758 \ud45c\uba74, \ubc18\uacbd \uc911\uac04, \uc911\uc2ec\uc5d0\uc11c \uce21\uc815\ud588\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud45c\uba74\uacfc \uc911\uc2ec\ubd80\uc758 \uacbd\ub3c4\uac00 \ub2e4\ub974\uac8c \ub098\ud0c0\ub098\ub294 \uc774\uc720\ub294 \ub0c9\uac01 \uc18d\ub3c4\uac00 \ub2e4\ub974\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uc544\ub798 \ub2e4\uc774\uc5b4\uadf8\ub7a8\uc740 \ub2e8\uba74\uc758 \ud45c\uba74\uc5d0\uc11c \uc911\uc2ec\ubd80\ub85c \uac08\uc218\ub85d \ub0c9\uac01 \uc18d\ub3c4\uac00 \uac10\uc18c\ud558\ub294 \ubaa8\uc2b5\uacfc \uadf8\uc5d0 \ub530\ub978 \ub0c9\uac01 \uace1\uc120\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Quenching-totten-fig-3-19-cooling-rate-over-section.jpg\" alt=\"Cooling rate falling from the surface to the centre of a quenched bar, with cooling curves at the surface, half radius and centre and the quenching and unquenching fields marked\"\/><figcaption class=\"wp-element-caption\">\uadf8\ub9bc 3.19. \ub2f4\uae08\uc9c8 \uc911 \uc2dc\ub8cc \ub2e8\uba74\uc758 \ub0c9\uac01 \uc18d\ub3c4. (a) \ub0c9\uac01 \uc18d\ub3c4\ub294 \ud45c\uba74\uc5d0\uc11c \uc784\uacc4 \uc18d\ub3c4(\ub2f4\uae08\uc9c8 \uc601\uc5ed) \uc774\uc0c1\uc5d0\uc11c \uc911\uc2ec\ubd80\uc758 \uc784\uacc4 \uc18d\ub3c4 \uc774\ud558(\ubbf8\ub2f4\uae08\uc9c8 \uc601\uc5ed)\ub85c \uac10\uc18c\ud569\ub2c8\ub2e4. (b) \uc6d0\ud615 \ubd09\uc758 \ud45c\uba74, \ubc18\uacbd \uc808\ubc18, \uc911\uc2ec\ubd80\uc5d0\uc11c\uc758 \ub0c9\uac01 \uace1\uc120\uacfc \uc624\ub978\ucabd\uc5d0 \uc2a4\ucf00\uce58\ub41c \ub2e8\uba74. \uc911\uc2ec \uace1\uc120\uc774 \uc784\uacc4 \uc18d\ub3c4 \uc774\ud558\ub85c \ub5a8\uc5b4\uc9c0\ub294 \uacf3\uc5d0\uc11c\ub294 \uc911\uc2ec\ubd80\uac00 \uc644\uc804\ud55c \uacbd\ub3c4\uc5d0 \ub3c4\ub2ec\ud558\uc9c0 \ubabb\ud558\uba70, \uc774\ub294 \uc544\ub798 \ud45c\uc758 \ud45c\uba74, \ubc18\uacbd \uc808\ubc18, \uc911\uc2ec\ubd80 \uce21\uc815\uac12\uc774 \ubcf4\uc5ec\uc8fc\ub294 \ubc14\uc785\ub2c8\ub2e4. \ucd9c\ucc98: A.V. Sverdlin and A.R. Ness, Fundamental Concepts in Steel Heat Treatment, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 3.19.<\/figcaption><\/figure>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc2dc\ud3b8<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud45c\uba74, HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubc18\uacbd \uc911\uac04, HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc911\uc2ec, HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 20 mm &times; 60 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc218\ub0c9<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 20 mm &times; 60 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">5% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">61<\/td><td class=\"has-text-align-left\" data-align=\"left\">57<\/td><td class=\"has-text-align-left\" data-align=\"left\">53<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 20 mm &times; 60 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">15% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">61<\/td><td class=\"has-text-align-left\" data-align=\"left\">57<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 20 mm &times; 60 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">25% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">58<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 20 mm &times; 60 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">L-AN15 \uc21c\uc720<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 30 mm &times; 90 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc218\ub0c9<\/td><td class=\"has-text-align-left\" data-align=\"left\">56<\/td><td class=\"has-text-align-left\" data-align=\"left\">33<\/td><td class=\"has-text-align-left\" data-align=\"left\">31<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 30 mm &times; 90 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">5% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">59<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">34<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 30 mm &times; 90 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">15% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">58<\/td><td class=\"has-text-align-left\" data-align=\"left\">38<\/td><td class=\"has-text-align-left\" data-align=\"left\">33<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 30 mm &times; 90 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">25% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><td class=\"has-text-align-left\" data-align=\"left\">33<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45\uac15, 30 mm &times; 90 mm<\/td><td class=\"has-text-align-left\" data-align=\"left\">L-AN15 \uc21c\uc720<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">23<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c 8-12, \uc778\uc1c4 \ud398\uc774\uc9c0 466. 45\uac15, 840\u00b0C\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ud558\uace0 30\ubd84 \uc720\uc9c0, \ub2e8\uba74 \uc804\uccb4\uc758 HRC \uacbd\ub3c4. 30 mm \ubd09\uc7ac\ub294 \ubaa8\ub4e0 \ub9e4\uccb4\uc5d0\uc11c \ubc18\uacbd \uc911\uac04\uacfc \uc911\uc2ec\uc5d0\uc11c \uc644\uc804 \uacbd\ub3c4\uc5d0 \ubbf8\uce58\uc9c0 \ubabb\ud569\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ubcc0\ud615 \ubc0f \ud45c\uba74 \uacbd\ub3c4<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\ubcc0\ud615 \uc2dc\ud5d8\uc5d0\ub294 50 mm \u00d7 10 mm 45\uac15 \ub514\uc2a4\ud06c\ub97c \uc0ac\uc6a9\ud588\uc73c\uba70, 840\u00b0C\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ud558\uace0 15\ubd84\uac04 \uc720\uc9c0\ud588\uc73c\uba70, \uce21\uc815\ub41c \ub514\uc2a4\ud06c\uc758 \uc131\uc7a5\ub7c9\uc774 \ud45c\uc758 \uc218\uce58\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uad50\ubc18\uc740 \uc791\uc5c5\uc7a5\uc5d0\uc11c \ub2f4\uae08\uc9c8 \uc911\uc5d0 \ubcc0\uacbd\ud560 \uc218 \uc788\ub294 \uc720\uc77c\ud55c \uacf5\uc815 \ubcc0\uc218\uc774\uba70, \uadf8 \ud6a8\uacfc\uc758 \ud06c\uae30\ub294 \ub9e4\uccb4\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-29-quenchant-velocity-cooling-curves.jpg\" alt=\"Effect of quenchant velocity on the centre cooling curves of an austenitic stainless steel specimen quenched into water at 60 C and into a 10% aqueous polymer solution at 30 C\"\/><figcaption class=\"wp-element-caption\">\uadf8\ub9bc 9.29. 25 mm &#215; 100 mm \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15 \uc2dc\ud3b8\uc744 (a) 60 &#176;C \ubb3c\uacfc (b) 30 &#176;C\uc758 10 % \uace0\ubd84\uc790 \uc218\uc6a9\uc561\uc5d0 0, 0.3, 0.6 m\/s\ub85c \ub2f4\uae08\uc9c8\ud588\uc744 \ub54c \uc911\uc2ec\ubd80 \ub0c9\uac01 \uace1\uc120\uc5d0 \ub300\ud55c \ub2f4\uae08\uc9c8\uc81c \uc720\uc18d\uc758 \uc601\ud5a5\uc785\ub2c8\ub2e4. \ubb3c\uc5d0\uc11c\ub294 \uc720\uc18d\uc774 \uc8fc\ub85c \uc99d\uae30\ub9c9 \ub2e8\uacc4\ub97c \ub2e8\ucd95\ud558\uace0 \uace1\uc120 \uc804\uccb4\ub97c \uc555\ucd95\ud569\ub2c8\ub2e4. \uace0\ubd84\uc790 \uc218\uc6a9\uc561\uc5d0\uc11c\ub294 \uace1\uc120 \ud558\ubd80\ub97c \ub290\ub9b0 \ub0c9\uac01 \uc601\uc5ed\uc5d0\uc11c \ub5bc\uc5b4\ub0b4\ub294 \uc5ed\ud560\ub3c4 \ud569\ub2c8\ub2e4. \uc608\uc2dc \uc18c\uc7ac\ub294 \ubcc0\ud0dc\ud558\uc9c0 \uc54a\uae30 \ub54c\ubb38\uc5d0 \uc120\ud0dd\ub41c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15\uc774\uba70, \ub530\ub77c\uc11c \uace1\uc120\uc740 \ub2f4\uae08\uc9c8\uc81c\ub9cc\uc744 \ubcf4\uc5ec \uc90d\ub2c8\ub2e4. \ucd9c\ucc98: H.M. Tensi, A. Stich \ubc0f G.E. Totten, Quenching and Quenching Technology, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 9.29.<\/figcaption><\/figure>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 \ubcc0\ud615, mm<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud45c\uba74 \uacbd\ub3c4, HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc218\ub0c9<\/td><td class=\"has-text-align-left\" data-align=\"left\">+0.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">+0.61<\/td><td class=\"has-text-align-left\" data-align=\"left\">61<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">15% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">+0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">25% NQ-1 \ud3f4\ub9ac\uba38<\/td><td class=\"has-text-align-left\" data-align=\"left\">+0.26<\/td><td class=\"has-text-align-left\" data-align=\"left\">58<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L-AN15 \uc21c\uc720<\/td><td class=\"has-text-align-left\" data-align=\"left\">+0.09<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c 8-13, \uc778\uc1c4 \ud398\uc774\uc9c0 466. 45\uac15 \ub514\uc2a4\ud06c, 50 mm \u00d7 10 mm, 840\u00b0C\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ud558\uace0 15\ubd84 \uc720\uc9c0. \ubcc0\ud615\uc740 \uce21\uc815\ub41c \ud06c\uae30 \ubcc0\ud654\uc758 \ud3c9\uade0\uc774\uba70, \uc591\uc218\ub294 \uc131\uc7a5\uc744 \uc758\ubbf8\ud569\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud45c\ub97c \ud568\uaed8 \uc77d\uae30<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ub2e4\uc12f \uac1c\uc758 \ud45c\uc5d0\uc11c \uc138 \uac00\uc9c0\uac00 \ub450\ub4dc\ub7ec\uc9d1\ub2c8\ub2e4. \ubb3c\uc740 \uade0\uc5f4 \uc2dc\ud5d8\uc5d0\uc11c \ubaa8\ub4e0 \uc2dc\ud3b8\uc5d0 \uade0\uc5f4\uc744 \uc77c\uc73c\ud0a4\uace0 \ubcc0\ud615 \ub514\uc2a4\ud06c\ub97c 0.80 mm \uc131\uc7a5\uc2dc\ucf30\uc73c\uba70, \ub450 \uad6c\uac04 \ubaa8\ub450\uc5d0\uc11c \uac00\uc7a5 \ube60\ub978 \ub9e4\uccb4\uc774\ubbc0\ub85c, \ubcc0\ud615\ub418\ub294 \uac15\uc885\uc5d0\uc11c\ub294 \ucd5c\ud6c4\uc758 \uc218\ub2e8 \ub9e4\uccb4\uc785\ub2c8\ub2e4. 15% \ud3f4\ub9ac\uba38 \ubc30\uc2a4\ub294 \uc2dc\ud3b8 \uc911 \uc5b4\ub290 \uac83\ub3c4 \uade0\uc5f4\uc2dc\ud0a4\uc9c0 \uc54a\uc558\uace0, \ubb3c\uacfc \ub3d9\uc77c\ud55c \ud45c\uba74 \ubc0f \uc911\uc2ec \uacbd\ub3c4\ub97c \uc720\uc9c0\ud588\uc73c\uba70, \ub514\uc2a4\ud06c\ub97c 0.12 mm\ub9cc \uc131\uc7a5\uc2dc\ucf30\ub294\ub370, \uc774\ub294 \uc138\ud2b8\uc5d0\uc11c \uac00\uc7a5 \uc881\uc740 \uacb0\uacfc\uc785\ub2c8\ub2e4. 25% \ubc30\uc2a4\ub294 \ub354 \ub2e8\ub2e8\ud55c \ubd09\uc7ac\uc5d0 \ub300\ud574 \ubcc0\ud615 \uba74\uc5d0\uc11c \uac00\uc7a5 \uc644\ub9cc\ud558\uace0 \ud45c\uba74\uc5d0\uc11c \uac00\uc7a5 \ubb34\ub974\uba70, \ub2e8\uba74 \uacbd\ub3c4\uac00 \uac00\uc7a5 \uba3c\uc800 \ub5a8\uc5b4\uc9c0\ubbc0\ub85c, \uadf8 \uc774\uc810\uc740 \uacbd\ub3c4\ubcf4\ub2e4 \ud615\uc0c1\uc5d0 \uc788\uc2b5\ub2c8\ub2e4. \uc21c\uc720\ub294 \uac00\uc7a5 \ub290\ub9ac\uace0 \uac00\uc7a5 \ubb34\ub974\uba70, \uc0c1\ubd80 \uad6c\uac04 \uc18d\ub3c4\uac00 \ucda9\ubd84\ud788 \ub0ae\uc544 \uc644\uc804 \ud569\uae08 \uac15\uc885\uc774 \ub4b7\ubc1b\uce68\ub418\uc5b4\uc57c \ud558\ub294 \ub9e4\uccb4\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uacbd\ub3c4\uc640 \ubcc0\ud615 \uc0ac\uc774\uc758 \uc808\ucda9\uc744 \uc561\uccb4\uc5d0\uc11c \uc804\ud600 \ud560 \uc218 \uc5c6\ub294 \uacbd\uc6b0, \uacf5\uae30 \uacbd\ud654 \uac15\uc885\uc774 \uadf8 \ubb38\uc81c\ub97c \uc5c6\uc560\uc8fc\uba70, \ub2e4\uc74c\uacfc \uac19\uc740 \uac15\uc774 <a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel\/\">D2<\/a> \ub294 \ubc30\uc2a4\uac00 \uc544\ub2cc \uc815\uc9c0 \uacf5\uae30 \ub610\ub294 \uac15\uc81c \uacf5\uae30 \ub2f4\uae08\uc9c8\uc5d0\uc11c \uc644\uc804 \uacbd\ub3c4\uc5d0 \ub3c4\ub2ec\ud569\ub2c8\ub2e4. \ubb3c\uc774 \uc5ec\uc804\ud788 \ud544\uc694\ud55c \uacbd\uc6b0, \ucd9c\ucc98\uc758 \uc8fc\uc11d\uc740 \ube60\ub978 \uc624\uc77c\uc774 \uc587\uac70\ub098 \ubd80\ubd84 \uc5f0\uc0ad\ub41c \ubd80\ud488\uc5d0\uc11c \uc885\uc885 \ubb3c\uc744 \ub300\uccb4\ud560 \uc218 \uc788\ub2e4\ub294 \uac83\uc774\uba70, \uc774\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/w1-tool-steel-heat-treatment\/\">W1<\/a> \uac00 \uc77c\ubc18\uc801\uc73c\ub85c \ucc44\ud0dd\ub418\ub294 \uacbd\ub85c\uc774\uba70 <a href=\"https:\/\/aobosteel.com\/ko\/o1-tool-steel\/\">O1<\/a> \uac00 \uc560\ucd08\uc5d0 \uc624\uc77c\uc6a9\uc73c\ub85c \ub9cc\ub4e4\uc5b4\uc9c4 \uc774\uc720\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ub370\uc774\ud130<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uac01 \uac15\uc885\uc5d0 \ud544\uc694\ud55c \ub2f4\uae08\uc9c8 \uc18d\ub3c4\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/quenching-chart-water-oil-air-hardening\/\">\uc218\ub0c9, \uc720\ub0c9 \ubc0f \uacf5\ub7ad \uacbd\ud654\uac15 \ub2f4\uae08\uc9c8 \ucc28\ud2b8<\/a>\uc5d0, \ud55c \uc5f4\uac04 \uac00\uacf5 \uac15\uc885\uc758 \uce21\uc815\ub41c \ub0c9\uac01 \uc18d\ub3c4\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/h13-quenching-cooling-rates\/\">H13 \ub2f4\uae08\uc9c8 \ub0c9\uac01 \uc18d\ub3c4 \ud398\uc774\uc9c0<\/a>\uc5d0, \uc804\uccb4 \uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1 \uc0ac\uc774\ud074\uc740 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-guide\/\">\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc<\/a>.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub370\uc774\ud130 \uad00\ub828 \ucc38\uace0\uc0ac\ud56d<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ub9e4\uccb4 \uc774\ub984\uc740 \ucd9c\ucc98\ub97c \ub530\ub985\ub2c8\ub2e4. \uc624\uc77c \ub4f1\uae09\uc740 \uc911\uad6d L-AN \uc804\uc190\uc2e4 \uc2dc\uc2a4\ud15c \uc624\uc77c\uc774\uba70, L-AN15\ub294 ISO VG15 \uc810\ub3c4 \ub4f1\uae09\uc5d0, L-AN32\ub294 ISO VG32\uc5d0 \uac00\uae4c\uc6b0\ubbc0\ub85c, \uc22b\uc790\ub294 \ube0c\ub79c\ub4dc\uac00 \uc544\ub2cc \uc810\ub3c4 \ub4f1\uae09\uc785\ub2c8\ub2e4. \ud3f4\ub9ac\uba38 \uc218\uce58\ub294 \ucd9c\ucc98 \uc2dc\ud5d8 \ud504\ub85c\uadf8\ub7a8\uc5d0 \uc0ac\uc6a9\ub41c NQ-1 \ud3f4\ub9ac\uba38\uc5d0 \ub300\ud55c \uac83\uc774\uba70 \ub18d\ub3c4\ub294 \uc9c8\ub7c9 \ubd84\uc728\uc774\ubbc0\ub85c, \ub2e4\ub978 \ud3f4\ub9ac\uba38\ub85c \uac19\uc740 \ube44\uc728\ub85c \ud63c\ud569\ud55c \ubc30\uc2a4\ub294 \ubc18\ub4dc\uc2dc \ub3d9\uc77c\ud558\uac8c \uac70\ub3d9\ud558\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \uade0\uc5f4, \uacbd\ud654\ub2a5 \ubc0f \ubcc0\ud615 \uc2dc\ud5d8\uc740 \ub2e4\uc774 \uac15\uc774 \uc544\ub2cc \ubcf4\ud1b5 \ud0c4\uc18c\uac15\uc778 T8 \ubc0f 45\uac15\uc5d0\uc11c \uc2e4\ud589\ub418\uc5c8\uc73c\ubbc0\ub85c, \uadf8 \ud310\ub3c5\uac12\uc740 \ub9e4\uccb4\ub97c \uce21\uc815\ud55c \uac83\uc774\uba70 \ud2b9\uc815 \uacf5\uad6c\uac15 \ub2e8\uba74\uc5d0 \ub300\ud55c \uc608\uce21\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc911\uad6d \uae08\ud615 \ubc0f \uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \ud578\ub4dc\ubd81, \ud45c 8-9\ubd80\ud130 8-13, \uc778\uc1c4 \ud398\uc774\uc9c0 464\ubd80\ud130 466\uc5d0\uc11c \ud3b8\uc9d1. \ud45c 8-9, 8-11, 8-12 \ubc0f 8-13\uc740 500 dpi\uc758 \ud398\uc774\uc9c0 \uc774\ubbf8\uc9c0\uc5d0\uc11c, \ud45c 8-10\uc740 \ud398\uc774\uc9c0 \uc774\ubbf8\uc9c0\uc640 \ud14d\uc2a4\ud2b8 \ub808\uc774\uc5b4\uc5d0\uc11c \ud310\ub3c5\ud588\uc2b5\ub2c8\ub2e4. \ud45c\ub294 Aobo Steel \uc0ac\uc591\uc774 \uc544\ub2cc \uacf5\uac1c\ub41c \uc2e4\ubb34\uc758 \ucc38\uc870 \uc694\uc57d\uc774\ubbc0\ub85c, \uc774\ub97c \uadfc\uac70\ub85c \uc8fc\ubb38\ud558\uae30 \uc804\uc5d0 \ubc00 \uc99d\uba85\uc11c\uc640 \ub300\uc870\ud558\uc5ec \ub9e4\uccb4\uc640 \uc0ac\uc774\ud074\uc744 \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uacf5\uad6c\uac15 \ub2f4\uae08\uc9c8 \ub9e4\uccb4, \uc778\uc1c4 \uac00\ub2a5 PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uc774 \ud398\uc774\uc9c0\uc758 \ub2e4\uc12f \uac1c \ud45c \ubaa8\ub450, \uc77c\ubc18 \ub9e4\uccb4\uc758 \ub0c9\uac01 \uc18d\ub3c4 \ubc0f \ud3f4\ub9ac\uba38 \uade0\uc5f4, \ub2e8\uba74 \uacbd\ub3c4 \ubc0f \ubcc0\ud615 \uacb0\uacfc\ub97c \ub2f9\uc0ac \uc5f0\ub77d\ucc98\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Quenching-Media-Cooling-Rates.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc<\/a><\/div>\n\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour A quench is judged by two numbers rather than one. The first is how fast the medium pulls heat out of the part in the range where pearlite and carbide would otherwise form, and the second is how fast it keeps cooling below the martensite [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20624","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Quenching Media for Tool Steel | Cooling Rates and Behaviour<\/title>\n<meta name=\"description\" content=\"Cooling rates of water, brine, caustic and oil quenchants for tool steel, with the cracking sensitivity, section hardness and distortion measured for a polymer quenchant at three concentrations.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/tool-steel-quenching-media-cooling-rates\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour\" \/>\n<meta property=\"og:description\" content=\"Cooling rates of water, brine, caustic and oil quenchants for tool steel, with the cracking sensitivity, section hardness and distortion measured for a polymer quenchant at three concentrations.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/tool-steel-quenching-media-cooling-rates\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:58:14+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"13\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour\",\"datePublished\":\"2026-10-02T21:09:15+00:00\",\"dateModified\":\"2026-10-15T16:58:14+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/\"},\"wordCount\":2636,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg\",\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/\",\"name\":\"Quenching Media for Tool Steel | Cooling Rates and Behaviour\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg\",\"datePublished\":\"2026-10-02T21:09:15+00:00\",\"dateModified\":\"2026-10-15T16:58:14+00:00\",\"description\":\"Cooling rates of water, brine, caustic and oil quenchants for tool steel, with the cracking sensitivity, section hardness and distortion measured for a polymer quenchant at three concentrations.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-quenching-media-cooling-rates\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uacf5\uad6c\uac15 \ub2f4\uae08\uc9c8 \ub9e4\uccb4 | \ub0c9\uac01 \uc18d\ub3c4 \ubc0f \uac70\ub3d9","description":"\uacf5\uad6c\uac15\uc6a9 \ubb3c, \uc5fc\uc218, \uc54c\uce7c\ub9ac \ubc0f \uc624\uc77c \ub2f4\uae08\uc9c8\uc81c\uc758 \ub0c9\uac01 \uc18d\ub3c4\uc640 3\uac1c \ub18d\ub3c4 \ud3f4\ub9ac\uba38 \ub2f4\uae08\uc9c8\uc81c\uc758 \uade0\uc5f4 \uac10\uc218\uc131, \ub2e8\uba74 \uacbd\ub3c4 \ubc0f \ubcc0\ud615 \uce21\uc815\uac12.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/tool-steel-quenching-media-cooling-rates\/","og_locale":"ko_KR","og_type":"article","og_title":"Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour","og_description":"Cooling rates of water, brine, caustic and oil quenchants for tool steel, with the cracking sensitivity, section hardness and distortion measured for a polymer quenchant at three concentrations.","og_url":"https:\/\/aobosteel.com\/ko\/tool-steel-quenching-media-cooling-rates\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:58:14+00:00","og_image":[{"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"13\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour","datePublished":"2026-10-02T21:09:15+00:00","dateModified":"2026-10-15T16:58:14+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/"},"wordCount":2636,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg","inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/","url":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/","name":"\uacf5\uad6c\uac15 \ub2f4\uae08\uc9c8 \ub9e4\uccb4 | \ub0c9\uac01 \uc18d\ub3c4 \ubc0f \uac70\ub3d9","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg","datePublished":"2026-10-02T21:09:15+00:00","dateModified":"2026-10-15T16:58:14+00:00","description":"\uacf5\uad6c\uac15\uc6a9 \ubb3c, \uc5fc\uc218, \uc54c\uce7c\ub9ac \ubc0f \uc624\uc77c \ub2f4\uae08\uc9c8\uc81c\uc758 \ub0c9\uac01 \uc18d\ub3c4\uc640 3\uac1c \ub18d\ub3c4 \ud3f4\ub9ac\uba38 \ub2f4\uae08\uc9c8\uc81c\uc758 \uade0\uc5f4 \uac10\uc218\uc131, \ub2e8\uba74 \uacbd\ub3c4 \ubc0f \ubcc0\ud615 \uce21\uc815\uac12.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/"]}]},{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Quenching-Media-totten-fig-9-27-film-boiling-heat-transfer-mechanism.jpg"},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-quenching-media-cooling-rates\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour A quench is judged by two numbers rather than one. The first is how fast the medium pulls heat out of the part in the range where pearlite and carbide would otherwise form, and the second is how fast it keeps cooling below the martensite&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Quenching Media for Tool Steel, Cooling Rates and Quenching Behaviour A quench is judged by two numbers rather than one. The first is how fast the medium pulls heat out of the part in the range where pearlite and carbide would otherwise form, and the second is how fast it keeps cooling below the martensite&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20624","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20624"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20624\/revisions"}],"predecessor-version":[{"id":22580,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20624\/revisions\/22580"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20624"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}