{"id":20489,"date":"2026-10-01T15:06:05","date_gmt":"2026-10-01T07:06:05","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20489"},"modified":"2026-10-16T00:46:19","modified_gmt":"2026-10-15T16:46:19","slug":"a2-a6-tool-steel-mechanical-properties","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/a2-a6-tool-steel-mechanical-properties\/","title":{"rendered":"\ud15c\ud37c\ub9c1 \ud6c4 A2 \ubc0f A6 \uacf5\uad6c\uac15\uc758 \uae30\uacc4\uc801 \uc131\uc9c8"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\ud15c\ud37c\ub9c1 \ud6c4 A2 \ubc0f A6 \uacf5\uad6c\uac15\uc758 \uae30\uacc4\uc801 \uc131\uc9c8<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\ud15c\ud37c\ub9c1\uc740 \ub0c9\uac04 \uac00\uacf5 \ub2e4\uc774\uc758 \uc2e4\uc81c \uc131\ub2a5\uc744 \uacb0\uc815\ud558\ub294 \ub2e8\uacc4\uc785\ub2c8\ub2e4. \uc65c\ub0d0\ud558\uba74 \uac15\uc885\uc774 \ub2f4\uae08\uc9c8 \ud6c4 \uac00\uc9c0\ub294 \uacbd\ub3c4\ub294 \uc2e4\uc81c \uc0ac\uc6a9 \uacbd\ub3c4\uac00 \uc544\ub2c8\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uc544\ub798 \ud45c\ub294 \ub450 \uac00\uc9c0 \uacf5\uae30 \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5 \uacf5\uad6c\uac15\uc778 A2\uc640 A6\uc5d0 \ub300\ud574 \uacbd\ub3c4, \uc778\uc7a5 \ubc0f \ud56d\ubcf5 \uac15\ub3c4, \uc5f0\uc2e0\uc728, \ub2e8\uba74 \uc218\ucd95\ub960, \ubb34\ub178\uce58 \uc0e4\ub974\ud53c \ucda9\uaca9\uac12\uc744 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uc640 \ud568\uaed8 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uac01 \uac15\uc885\uc740 \ud45c \uc544\ub798\uc5d0 \uba85\uc2dc\ub41c \ub2f4\uae08\uc9c8 \uc628\ub3c4\uc5d0\uc11c \ud558\ub098\uc758 \ud788\ud2b8\ub85c \ucc98\ub9ac\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \ubaa8\ub4e0 \uc218\uce58\ub294 \uc606\uc5d0 \ud45c\uc2dc\ub41c \uc815\ud655\ud55c \ub2f4\uae08\uc9c8 \ubc0f \ud15c\ud37c\ub9c1 \uc870\uac74\uc5d0 \ud574\ub2f9\ud558\ubbc0\ub85c, \uc124\uacc4\uac12\uc774 \uc544\ub2cc \uce21\uc815\ub41c \uac70\ub3d9\uc73c\ub85c \uc77d\uc5b4\uc57c \ud569\ub2c8\ub2e4. \uc774\ub294 \uacf5\uac1c\ub41c \uc2e4\ubb34\uc5d0 \ub300\ud55c \ucc38\uace0 \uc694\uc57d\uc774\uba70 \ub2f9\uc0ac\uc758 \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc218\uce58\uac00 \uce21\uc815\ud558\ub294 \uac83<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud45c\uc5d0 \uc788\ub294 \ub450 \uac15\uc885\uc740 \ub2f4\uae08\uc9c8 \ud6c4 \ud55c \ubc88 \ud15c\ud37c\ub9c1\ud558\ub294 \uacf5\uae30 \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5 \uac15\uc885\uc774\uba70, \uc5f4 \uc804\uccb4\uc5d0\uc11c \uc720\uc77c\ud55c \ubcc0\uc218\ub294 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uc785\ub2c8\ub2e4. A2\ub294 945 &#176;C (1730 &#176;F)\uc5d0\uc11c \ub2f4\uae08\uc9c8\ub418\uc5c8\uace0 540 \ubc0f 595 &#176;C\uc758 \ub450 \uac00\uc9c0 \ud15c\ud37c\ub9c1 \uc628\ub3c4\ub85c \ucc98\ub9ac\ub418\uc5c8\uc2b5\ub2c8\ub2e4. A6\ub294 845 &#176;C (1550 &#176;F)\uc5d0\uc11c \ub2f4\uae08\uc9c8\ub418\uc5c8\uace0 175, 315 \ubc0f 480 &#176;C\uc758 \uc138 \uac00\uc9c0 \uc628\ub3c4\ub85c \ucc98\ub9ac\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uacbd\ub3c4, \ucd5c\ub300 \uac15\ub3c4 \ubc0f \uc5f0\uc131 \uce21\uc815\uac12\uc740 \uc774 \ub2e8\uc77c \ud15c\ud37c\ub9c1\uc758 \uacb0\uacfc\uc774\ubbc0\ub85c, \uc774 \ud45c\ub294 \ub2e4\uc774 \uacf5\uc7a5\uc5d0\uc11c \ud380\uce58, \ub2e4\uc774 \uc778\uc11c\ud2b8 \ub610\ub294 \uc808\uc0ad\ub0a0\uc5d0 \ub300\ud55c \ud15c\ud37c\ub9c1 \uc628\ub3c4\ub97c \uc120\ud0dd\ud560 \ub54c \ubb3b\ub294 \uc9c8\ubb38\uc5d0 \ub2f5\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub450 \uac15\uc885\uc740 \ub3d9\uc77c\ud55c \uae4a\uc774\ub85c \uc2dc\ud5d8\ub418\uc9c0 \uc54a\uc558\uc2b5\ub2c8\ub2e4. \ucd9c\ucc98\ub294 A2\uc5d0 \ub300\ud574 \uacbd\ub3c4\uc640 \ucd5c\ub300 \uac15\ub3c4\ub97c \ubcf4\uace0\ud558\uace0 \ud56d\ubcf5 \uac15\ub3c4, \uc5f0\uc2e0\uc728, \ub2e8\uba74 \uc218\ucd95\ub960 \ubc0f \ucda9\uaca9 \uc5f4\uc744 \ube44\uc6cc \ub450\uc5c8\uc73c\uba70, \uc5ec\uae30\uc11c\ub294 \ucd9c\ucc98\uac00 \uc778\uc1c4\ud55c \uadf8\ub300\ub85c \uc138 \uac1c\uc758 \uc810\uc73c\ub85c \ud45c\uc2dc\ud588\uc2b5\ub2c8\ub2e4. A6\ub294 \ub178\uce58 \uc2dc\ud5d8\uc744 \uc81c\uc678\ud558\uace0 \ubb34\ub178\uce58 \uc0e4\ub974\ud53c \uac12\uc774 \uc81c\uacf5\ub418\uc5b4 \uc804\uccb4\uc801\uc73c\ub85c \ucc98\ub9ac\ub418\uc5c8\uc73c\uba70, \uc774\ub294 \ub9c8\uc9c0\ub9c9 \ub450 \uc5f4\uc774 \ub178\uce58 \ucda9\uaca9 \ud310\ub3c5\uac12\ubcf4\ub2e4 \ub354 \ud070 \uc22b\uc790\ub97c \uac00\uc9c0\ub294 \uc774\uc720\uc785\ub2c8\ub2e4. \ub610\ud55c A6\ub294 175 &#176;C\uc5d0\uc11c \ubcf4\uace0\ub418\uc5c8\ub294\ub370, \uc774\ub294 \ubaa8\ub4e0 \ud15c\ud37c\ub9c1 \ubc94\uc704\uc758 \ub0ae\uc740 \ub05d\uc5d0 \ud574\ub2f9\ud558\uba70 \uc5f0\ud654\uac00 \uc544\ub2cc \uc751\ub825 \uc81c\uac70 \uc911\uc778 \ubd80\ud488\uc5d0 \uc18d\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud15c\ud37c\ub9c1 \ud6c4 \uacbd\ub3c4, \uac15\ub3c4 \ubc0f \ucda9\uaca9<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">945 &#176;C (1730 &#176;F)\uc5d0\uc11c \ub2f4\uae08\uc9c8\ud558\uace0 \ud55c \ubc88 \ud15c\ud37c\ub9c1\ud55c \ud6c4\uc758 A2 \uacf5\uad6c\uac15<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4, &#176;C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4, &#176;F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4, HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \uac15\ub3c4, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \uac15\ub3c4, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud56d\ubcf5 \uac15\ub3c4, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud56d\ubcf5 \uac15\ub3c4, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">50 mm (2 in.)\uc5d0\uc11c\uc758 \uc5f0\uc2e0\uc728, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \uc218\ucd95\ub960, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubb34\ub178\uce58 \uc0e4\ub974\ud53c \ucda9\uaca9, J<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubb34\ub178\uce58 \uc0e4\ub974\ud53c \ucda9\uaca9, ft&#183;lbf<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">540<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1858.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">269.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">595<\/td><td class=\"has-text-align-left\" data-align=\"left\">1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">46.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">1603.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">232.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">1269<\/td><td class=\"has-text-align-left\" data-align=\"left\">184<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, Tool Steels (G. A. Roberts and G. Krauss), \ud45c 11-3, A2 \ubc0f A6 \uacf5\uad6c\uac15\uc758 \uae30\uacc4\uc801 \uc131\uc9c8, \uc778\uc1c4 \ud398\uc774\uc9c0 199. A2 \uc218\uce58\ub294 Teledyne VASCO\uc5d0\uc11c \uc81c\uacf5. \uc138 \uac1c\uc758 \uc810\uc740 \ucd9c\ucc98\uac00 \ud574\ub2f9 \uc131\uc9c8\uc5d0 \ub300\ud55c \uc218\uce58\ub97c \uc81c\uacf5\ud558\uc9c0 \uc54a\ub294 \uacf3\uc5d0 \uc778\uc1c4\ud55c \uac83\uc785\ub2c8\ub2e4. \uc774\ub294 \uacf5\uac1c\ub41c \uc2e4\ubb34\uc5d0 \ub300\ud55c \ucc38\uace0 \uc694\uc57d\uc774\uba70 Aobo Steel \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h3 class=\"wp-block-heading\">845 &#176;C (1550 &#176;F)\uc5d0\uc11c \ub2f4\uae08\uc9c8\ud558\uace0 \ud55c \ubc88 \ud15c\ud37c\ub9c1\ud55c \ud6c4\uc758 A6 \uacf5\uad6c\uac15<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4, &#176;C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4, &#176;F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4, HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \uac15\ub3c4, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \uac15\ub3c4, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud56d\ubcf5 \uac15\ub3c4, MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud56d\ubcf5 \uac15\ub3c4, ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">50 mm (2 in.)\uc5d0\uc11c\uc758 \uc5f0\uc2e0\uc728, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \uc218\ucd95\ub960, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubb34\ub178\uce58 \uc0e4\ub974\ud53c \ucda9\uaca9, J<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubb34\ub178\uce58 \uc0e4\ub974\ud53c \ucda9\uaca9, ft&#183;lbf<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">175<\/td><td class=\"has-text-align-left\" data-align=\"left\">350<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">2137<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">117<\/td><td class=\"has-text-align-left\" data-align=\"left\">86<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">55.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2016.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">292.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1822.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">264.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">163<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">900<\/td><td class=\"has-text-align-left\" data-align=\"left\">51.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1751<\/td><td class=\"has-text-align-left\" data-align=\"left\">254<\/td><td class=\"has-text-align-left\" data-align=\"left\">1510<\/td><td class=\"has-text-align-left\" data-align=\"left\">219<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, Tool Steels (G. A. Roberts and G. Krauss), \ud45c 11-3, \uc778\uc1c4 \ud398\uc774\uc9c0 199. A6 \uc218\uce58\ub294 Universal Cyclops Steel Corp.\uc5d0\uc11c \uc81c\uacf5. \ucda9\uaca9 \uc5f4\uc740 \ubb34\ub178\uce58 \uc0e4\ub974\ud53c\uc774\ubbc0\ub85c \ub3d9\uc77c \uac15\uc885\uc758 \ub178\uce58 \ud310\ub3c5\uac12\uacfc \ube44\uad50\ud560 \uc218 \uc5c6\uc73c\uba70, 175 &#176;C\ub294 \uc5f0\ud654\uac00 \uc544\ub2cc \uc751\ub825 \uc81c\uac70 \ud15c\ud37c\ub9c1\uc785\ub2c8\ub2e4. \uc774\ub294 \uacf5\uac1c\ub41c \uc2e4\ubb34\uc5d0 \ub300\ud55c \ucc38\uace0 \uc694\uc57d\uc774\uba70 Aobo Steel \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub450 \uac15\uc885\uc744 \ud568\uaed8 \uc77d\uae30<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uba3c\uc800 \uacbd\ub3c4 \uc5f4\uc744 \ubcf4\uc2ed\uc2dc\uc624. A2\ub294 \ub450 \uc870\uac74\uc5d0\uc11c 54.1\uc5d0\uc11c 46.7 HRC\ub85c \ub5a8\uc5b4\uc9c0\uba70, 55 &#176;C \ub354 \ud15c\ud37c\ub9c1\ud560 \ub54c 7.4 \ud3ec\uc778\ud2b8 \ud558\ub77d\ud558\uace0, \ucd5c\ub300 \uac15\ub3c4\ub3c4 1858.2\uc5d0\uc11c 1603.8 MPa\ub85c \ub530\ub77c \ub0b4\ub824\uac11\ub2c8\ub2e4. \uc774 \ub2e8\uc77c \ub2e8\uacc4\uac00 \uacbd\ud654\ub41c \ub0a0\uacfc \uc778\uc131 \uc788\ub294 \ub0a0 \uc0ac\uc774\uc5d0\uc11c \uacb0\uc815\ud560 \ub54c \uacf5\uc7a5\uc774 A2\uc5d0 \ub300\ud574 \ud558\ub294 \uc804\uccb4 \ud2b8\ub808\uc774\ub4dc\uc624\ud504\uc774\uba70, \ucd9c\ucc98\ub294 \uadf8 \ubc18\ub300\ud3b8\uc758 \uac00\uaca9\uc744 \ub9e4\uae38 \ucda9\uaca9 \uc218\uce58\ub97c \uc81c\uacf5\ud558\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A6\ub294 \ucda9\uaca9 \uce21\uba74\uc774 \ucc44\uc6cc\uc9c4 \ub3d9\uc77c\ud55c \ud2b8\ub808\uc774\ub4dc\uc624\ud504\ub97c \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \ud15c\ud37c\ub9c1 \uc628\ub3c4\uac00 175\uc5d0\uc11c 315\ub85c 480 &#176;C\ub85c \uac08 \ub54c \uacbd\ub3c4\ub294 59.7, 55.5, 51.0 HRC\ub85c \ub5a8\uc5b4\uc9c0\uace0, \ubb34\ub178\uce58 \uc0e4\ub974\ud53c \uc5d0\ub108\uc9c0\ub294 117, 163, 170 J\ub85c \uc0c1\uc2b9\ud558\uba70, \uc5f0\uc2e0\uc728\uc740 0.5\uc5d0\uc11c 2.5 \ud37c\uc13c\ud2b8\ub85c \uc0c1\uc2b9\ud558\uace0 \ub2e8\uba74 \uc218\ucd95\ub960\uc740 1.0\uc5d0\uc11c 7.4 \ud37c\uc13c\ud2b8\ub85c \uac11\ub2c8\ub2e4. \uacbd\ub3c4 \uc190\uc2e4\uc774 \uac00\uc7a5 \uc791\uc73c\uba74\uc11c \uc778\uc131\uc758 \uac00\uc7a5 \ud070 \ub2e8\uc77c \uc774\ub4dd\uc740 175\uc640 315 &#176;C \uc0ac\uc774\uc5d0 \uc788\uc73c\uba70, \uc5ec\uae30\uc11c 4.2 HRC\uac00 46 J\ub97c \uc0bd\ub2c8\ub2e4. \uadf8 \uc774\ud6c4\ub85c \uace1\uc120\uc740 \ud3c9\ud3c9\ud574\uc9c0\uace0, 315\uc5d0\uc11c 480 &#176;C\ub85c\uc758 \ub2e8\uacc4\ub294 7 J\uc5d0 \ub300\ud574 \ub610 \ub2e4\ub978 4.5 HRC\ub97c \uc18c\ubaa8\ud558\uba70, \uc774\ub294 \uacf5\uc7a5\uc774 \ubcf4\ud1b5 \uba48\ucd94\uace0 \ub354 \uacbd\ud654\ub41c \uc870\uac74\uc744 \ubc1b\uc544\ub4e4\uc774\ub294 \uc9c0\uc810\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud56d\ubcf5 \uc218\uce58\ub294 \ud55c \uac00\uc9c0 \uc8fc\uc758\uac00 \ud544\uc694\ud569\ub2c8\ub2e4. 315 &#176;C \uc870\uac74\uc758 A6\ub294 \ucd5c\ub300 \uac15\ub3c4 2016.8 MPa\uc5d0 \ub300\ud574 \ud56d\ubcf5 \uac15\ub3c4 1822.3 MPa\ub85c \uc778\uc1c4\ub418\uc5b4 \uc788\uc73c\uba70, \uc774 \ube44\uc728\uc740 \ud56d\ubcf5\uacfc \ud30c\uad34 \uc0ac\uc774\uc5d0 \ub9e4\uc6b0 \uc801\uc740 \uc5ec\uc720\ub97c \ub0a8\uae30\uace0, 480 &#176;C\uc5d0\uc11c \ub3d9\uc77c \uac15\uc885\uc740 \uadf8 \uac04\uaca9\uc744 241 MPa\ub85c \ubc8c\ub9bd\ub2c8\ub2e4. \ub530\ub77c\uc11c \ub354 \uacbd\ud654\ub418\uace0 \ub0ae\uc740 \uc628\ub3c4 \uc870\uac74\uc5d0\uc11c \uc791\ub3d9\ud558\ub294 \ub2e4\uc774\ub294 \uade0\uc5f4 \uc804\uc5d0 \uac70\uc758 \uc5ec\uc720\uac00 \uc5c6\uc73c\uba70, \uc774\ub294 \uc606\uc5d0 \uc778\uc1c4\ub41c \ub9e4\uc6b0 \ub0ae\uc740 \uc5f0\uc2e0\uc728 \ubc0f \ub2e8\uba74 \uc218\ucd95\ub960\uacfc \uc77c\uce58\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ub370\uc774\ud130<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ub0c9\uac04 \uac00\uacf5 \ud1a4\uc218\uc758 \ub300\ubd80\ubd84\uc744 \ucc28\uc9c0\ud558\ub294 \uac15\uc885\uc740 \uadf8 \ud615\ud0dc, \ub2e8\uba74 \ubc94\uc704 \ubc0f \ub0a9\ud488 \uc870\uac74\uc774 \ub2e4\uc74c\uc5d0 \uc124\uba85\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel\/\">A2 \uacf5\uad6c\uac15<\/a>, \uadf8\ub9ac\uace0 \ub3d9\uc77c \uac15\uc885\uc758 \uc131\uc9c8, \uacbd\ub3c4 \ubc94\uc704 \ubc0f \uc6a9\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel-properties\/\">A2 \uacf5\uad6c\uac15 \ud2b9\uc131<\/a> \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel-hardness\/\">A2 \uacf5\uad6c\uac15 \uacbd\ub3c4<\/a>. \uc804\uccb4 \uacf5\uae30 \uacbd\ud654 \uadf8\ub8f9\uc758 \ub2f4\uae08\uc9c8 \ubc0f \ud15c\ud37c\ub9c1 \ubc94\uc704\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc73c\uba70 <a href=\"https:\/\/aobosteel.com\/ko\/air-hardening-tool-steel\/\">\uacf5\uae30 \uacbd\ud654 \uacf5\uad6c\uac15<\/a>, \uac01 \uacf5\uad6c\uac15 \uac15\uc885\uc774 \uc8fc\uc5b4\uc9c4 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uc5d0\uc11c \uc720\uc9c0\ud558\ub294 \uacbd\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \ucc28\ud2b8\ub85c \ud45c\uc2dc\ub418\uc5b4 \uc788\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-tempering-chart\/\">\uacf5\uad6c\uac15 \ud15c\ud37c\ub9c1 \ucc28\ud2b8<\/a>, \uacf5\uad6c\uac15 \uac15\uc885\uc758 \ucda9\uaca9 \uac12\uc740 \ub2e4\uc74c\uc5d0 \uc218\uc9d1\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-impact-toughness-chart\/\">\uacf5\uad6c\uac15 \ucda9\uaca9 \uc778\uc131<\/a>. \uce58\ud551\uc5d0 \uc800\ud56d\ud574\uc57c \ud558\ub294 \uacf5\uad6c\uc758 \ud15c\ud37c\ub9c1 \uc628\ub3c4 \uc120\ud0dd \ubc29\ubc95\uc740 \ub2e4\uc74c\uc5d0\uc11c \ub2e4\ub8e8\uc5b4\uc9d1\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steels-for-chipping-resistance\/\">\uce58\ud551 \uc800\ud56d\uc131 \uacf5\uad6c\uac15<\/a>.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>A2 \ubc0f A6 \uacf5\uad6c\uac15 \uae30\uacc4\uc801 \uc131\uc9c8, \uc778\uc1c4 \uac00\ub2a5\ud55c PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">175\uc5d0\uc11c 595 &#176;C\uae4c\uc9c0 \ud15c\ud37c\ub9c1\ud55c \ud6c4 A2 \ubc0f A6 \ub0c9\uac04 \uac00\uacf5 \uacf5\uad6c\uac15\uc758 \uacbd\ub3c4, \ucd5c\ub300 \ubc0f \ud56d\ubcf5 \uac15\ub3c4, \uc5f0\uc2e0\uc728, \ub2e8\uba74 \uc218\ucd95\ub960 \ubc0f \ubb34\ub178\uce58 \uc0e4\ub974\ud53c \ucda9\uaca9\uc744 \ub2f9\uc0ac \uc5f0\ub77d\ucc98\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-A2-A6-Tool-Steel-Mechanical-Properties.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">\uacf5\uae30 \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5 \uacf5\uad6c\uac15\uc5d0 \uad00\ud55c \uc7a5\uc778 Tool Steels (G. A. Roberts and G. Krauss), \ud45c 11-3, A2 \ubc0f A6 \uacf5\uad6c\uac15\uc758 \uae30\uacc4\uc801 \uc131\uc9c8, \uc778\uc1c4 \ud398\uc774\uc9c0 199\uc5d0\uc11c \ud3b8\uc9d1\ud588\uc2b5\ub2c8\ub2e4. \ud45c\ub294 \ucd9c\ud310\ub41c \ub300\ub85c \uc7ac\ud604\ub418\uc5c8\uc73c\uba70 Aobo Steel \uaddc\uaca9\uc774 \uc544\ub2cc \ucc38\uace0 \uc694\uc57d\uc774\ubbc0\ub85c, \ud2b9\uc815 \ub2e4\uc774\uc5d0 \ub300\ud55c \uc124\uacc4 \ud5c8\uc6a9\uac12\uc774 \uc544\ub2cc \ud558\ub098\uc758 \ud788\ud2b8\uac00 \ud558\ub098\uc758 \uc5f4\ucc98\ub9ac \ud558\uc5d0\uc11c \ubcf4\uc774\ub294 \uce21\uc815\ub41c \uac70\ub3d9\uc73c\ub85c \ucde8\uae09\ud558\uc2ed\uc2dc\uc624.<\/p>","protected":false},"excerpt":{"rendered":"<p>A2 and A6 Tool Steel Mechanical Properties After Tempering Tempering is the step that decides what a cold work die can actually take, because the hardness a grade leaves the quench with is not the hardness it works at. The table below sets hardness, tensile and yield strength, elongation, reduction of area and unnotched Charpy [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20489","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>A2 and A6 Tool Steel Properties by Tempering Temperature<\/title>\n<meta name=\"description\" content=\"Measured hardness, tensile and yield strength, elongation, reduction of area and unnotched Charpy impact of A2 and A6 cold work tool steels after tempering.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/a2-a6-tool-steel-mechanical-properties\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"A2 and A6 Tool Steel Mechanical Properties After Tempering\" \/>\n<meta property=\"og:description\" content=\"Measured hardness, tensile and yield strength, elongation, reduction of area and unnotched Charpy impact of A2 and A6 cold work tool steels after tempering.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/a2-a6-tool-steel-mechanical-properties\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:46:19+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"5\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a2-a6-tool-steel-mechanical-properties\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a2-a6-tool-steel-mechanical-properties\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"A2 and A6 Tool Steel Mechanical Properties After Tempering\",\"datePublished\":\"2026-10-01T07:06:05+00:00\",\"dateModified\":\"2026-10-15T16:46:19+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a2-a6-tool-steel-mechanical-properties\\\/\"},\"wordCount\":1049,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a2-a6-tool-steel-mechanical-properties\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/a2-a6-tool-steel-mechanical-properties\\\/\",\"name\":\"A2 and A6 Tool Steel Properties by Tempering Temperature\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-01T07:06:05+00:00\",\"dateModified\":\"2026-10-15T16:46:19+00:00\",\"description\":\"Measured hardness, tensile and yield strength, elongation, reduction of area and unnotched Charpy impact of A2 and A6 cold work tool steels after tempering.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a2-a6-tool-steel-mechanical-properties\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/a2-a6-tool-steel-mechanical-properties\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a2-a6-tool-steel-mechanical-properties\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"A2 and A6 Tool Steel Mechanical Properties After Tempering\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\ub728\uc784 \uc628\ub3c4\ubcc4 A2, A6 \uacf5\uad6c\uac15 \ud2b9\uc131","description":"A2 \ubc0f A6 \ub0c9\uac04 \uae08\ud615\uc6a9 \uacf5\uad6c\uac15\uc758 \ud15c\ud37c\ub9c1 \ud6c4 \uacbd\ub3c4, \uc778\uc7a5\uac15\ub3c4, \ud56d\ubcf5\uac15\ub3c4, \uc5f0\uc2e0\uc728, \ub2e8\uba74\uc218\ucd95\ub960 \ubc0f \ubb34\ub178\uce58 \uc0e4\ub974\ud53c \ucda9\uaca9\uac12\uc744 \uce21\uc815\ud55c \uacb0\uacfc\uc785\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/a2-a6-tool-steel-mechanical-properties\/","og_locale":"ko_KR","og_type":"article","og_title":"A2 and A6 Tool Steel Mechanical Properties After Tempering","og_description":"Measured hardness, tensile and yield strength, elongation, reduction of area and unnotched Charpy impact of A2 and A6 cold work tool steels after tempering.","og_url":"https:\/\/aobosteel.com\/ko\/a2-a6-tool-steel-mechanical-properties\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:46:19+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"5\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/a2-a6-tool-steel-mechanical-properties\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/a2-a6-tool-steel-mechanical-properties\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"A2 and A6 Tool Steel Mechanical Properties After Tempering","datePublished":"2026-10-01T07:06:05+00:00","dateModified":"2026-10-15T16:46:19+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/a2-a6-tool-steel-mechanical-properties\/"},"wordCount":1049,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/a2-a6-tool-steel-mechanical-properties\/","url":"https:\/\/aobosteel.com\/a2-a6-tool-steel-mechanical-properties\/","name":"\ub728\uc784 \uc628\ub3c4\ubcc4 A2, A6 \uacf5\uad6c\uac15 \ud2b9\uc131","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-01T07:06:05+00:00","dateModified":"2026-10-15T16:46:19+00:00","description":"A2 \ubc0f A6 \ub0c9\uac04 \uae08\ud615\uc6a9 \uacf5\uad6c\uac15\uc758 \ud15c\ud37c\ub9c1 \ud6c4 \uacbd\ub3c4, \uc778\uc7a5\uac15\ub3c4, \ud56d\ubcf5\uac15\ub3c4, \uc5f0\uc2e0\uc728, \ub2e8\uba74\uc218\ucd95\ub960 \ubc0f \ubb34\ub178\uce58 \uc0e4\ub974\ud53c \ucda9\uaca9\uac12\uc744 \uce21\uc815\ud55c \uacb0\uacfc\uc785\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/a2-a6-tool-steel-mechanical-properties\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/a2-a6-tool-steel-mechanical-properties\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/a2-a6-tool-steel-mechanical-properties\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"A2 and A6 Tool Steel Mechanical Properties After Tempering"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"A2 and A6 Tool Steel Mechanical Properties After Tempering Tempering is the step that decides what a cold work die can actually take, because the hardness a grade leaves the quench with is not the hardness it works at. The table below sets hardness, tensile and yield strength, elongation, reduction of area and unnotched Charpy&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"A2 and A6 Tool Steel Mechanical Properties After Tempering Tempering is the step that decides what a cold work die can actually take, because the hardness a grade leaves the quench with is not the hardness it works at. The table below sets hardness, tensile and yield strength, elongation, reduction of area and unnotched Charpy&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20489","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20489"}],"version-history":[{"count":2,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20489\/revisions"}],"predecessor-version":[{"id":22554,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20489\/revisions\/22554"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20489"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}