{"id":20442,"date":"2026-10-01T09:11:55","date_gmt":"2026-10-01T01:11:55","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20442"},"modified":"2026-10-16T00:40:35","modified_gmt":"2026-10-15T16:40:35","slug":"tool-steel-fracture-toughness-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/tool-steel-fracture-toughness-chart\/","title":{"rendered":"\uacf5\uad6c\uac15 \ud30c\uad34\uc778\uc131 \ucc28\ud2b8 (K1c)"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\uacf5\uad6c\uac15 \ud30c\uad34\uc778\uc131 \ucc28\ud2b8 (K1c)<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">8\uac00\uc9c0 \uc77c\ubc18 \uacf5\uad6c\uac15 \ub4f1\uae09\uc5d0 \ub300\ud55c MPa root metre \ub2e8\uc704\uc758 \ud30c\uad34\uc778\uc131\uc73c\ub85c, \uc138 \uac00\uc9c0 \ub2e8\uc870 \uc555\ud558\uc728\uc5d0\uc11c \ucc44\ucde8\ud55c \uad7d\ud798 \uc2dc\ud3b8\uc744 \uc138 \uac00\uc9c0 \uc628\ub3c4\uc5d0\uc11c \ud15c\ud37c\ub9c1\ud558\uc5ec \uce21\uc815\ud558\uc600\uc73c\uba70, \uac01 \uc2dc\ud3b8\uc774 \uc2dc\ud5d8\ub41c \uacbd\ub3c4\ub97c \ud568\uaed8 \ud45c\uc2dc\ud558\uc600\ub2e4. \uacf5\uac1c\ub41c \uc2e4\ubb34\ub97c \uc694\uc57d\ud55c \ucc38\uace0 \uc790\ub8cc\uc774\uba70 Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uac12\uc758 \ud68d\ub4dd \ubc29\ubc95<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \ud398\uc774\uc9c0\uc758 \ubaa8\ub4e0 \uc218\uce58\ub294 \ub3d9\uc77c\ud55c 8\uac00\uc9c0 \ub4f1\uae09\uc5d0 \ub300\ud574 \uc138 \uac00\uc9c0 \uc778\uc131 \uc2dc\ud5d8\uc744 \ub3d9\uc2dc\uc5d0 \uc218\ud589\ud55c \ud558\ub098\uc758 \uc2e4\ud5d8\uc2e4 \ud504\ub85c\uadf8\ub7a8\uc5d0\uc11c \ub098\uc628 \uac83\uc774\ubbc0\ub85c \uc11c\ub85c \ube44\uad50\ud558\uc5ec \uc77d\uc744 \uc218 \uc788\ub2e4. \uac15\uc7ac\ub294 432 mm \uc6d0\ud615 \uc804\uae30\uc2ac\ub798\uadf8 \uc7ac\uc6a9\ud574 \uc789\uacf3\uc73c\ub85c \uacf5\uae09\ub418\uc5c8\ub2e4. \uac01 \ub4f1\uae09\uc758 \uc2dc\ub8cc\ub294 146~173 mm \uc6d0\ud615 \ubd09\uc5d0\uc11c \uc808\ub2e8\ub418\uc5c8\uace0, \uac01 \uc2dc\ub8cc\uc758 \uc77c\ubd80\ub294 89 mm \uc815\uc0ac\uac01\ud615 \ubc0f 38 mm \uc815\uc0ac\uac01\ud615\uc73c\ub85c \ub2e8\uc870\ub418\uc5c8\uc73c\uba70, \uc774\ub294 88, 95, 99 \ud37c\uc13c\ud2b8\ub85c \uae30\uc7ac\ub41c \uc138 \uac00\uc9c0 \ucd1d \ub2e8\uc870 \uc555\ud558\uc728\uc744 \uc81c\uacf5\ud55c\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud30c\uad34\uc778\uc131\uc740 114 mm x 25 mm x 13 mm\uc758 \ud45c\uc900 \uad7d\ud798 \uc2dc\ud3b8\uc73c\ub85c \uce21\uc815\ub418\uc5c8\uc73c\uba70, 25 mm \uce58\uc218\uc5d0\uc11c \uc57d\uac04 \ud06c\uac8c \uac00\uacf5\ud558\uace0, \ub178\uce58\ub97c \ub123\uace0, \uc5f4\ucc98\ub9ac\ud55c \ud6c4 \uc2e4\uc628\uc5d0\uc11c \uc2dc\ud5d8\ud558\uae30 \uc804\uc5d0 \ucd5c\uc885 \uac00\uacf5\ud558\uc600\ub2e4. \uac01 \ub4f1\uae09\ub2f9 \uc138 \uac00\uc9c0 \ud15c\ud37c\ub9c1 \uc628\ub3c4 \uac01\uac01\uc5d0\uc11c 2\uac1c \ubc0f \uc77c\ubd80 3\uac1c \uc2dc\ud3b8\uc744 \ud15c\ud37c\ub9c1\ud558\uc600\uc73c\uba70, \uc774 \ub54c\ubb38\uc5d0 \ub300\ubd80\ubd84\uc758 \ud589\uc5d0 \ub450 \uac1c\uc758 \uc2dc\ud5d8\uac12\uc774 \uc788\uace0 H13 \ud589\uc5d0\ub294 \uc138 \uac1c\uac00 \uc788\ub2e4. \uacbd\ub3c4\ub294 \uc2dc\ud5d8 \ud6c4 \ubaa8\ub4e0 \uc2dc\ud3b8\uc5d0\uc11c \uce21\uc815\ub418\uc5c8\uc73c\ubbc0\ub85c HRC \uc5f4\uc740 \uacf5\uce6d \uc218\uce58\uac00 \uc544\ub2c8\ub77c \ud574\ub2f9 \uc2dc\ud3b8\uc774 \uc2e4\uc81c\ub85c \uc2dc\ud5d8\ub41c \uacbd\ub3c4\uc774\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc778\uc131 \uac12\uc740 MPa root metre\ub85c \uc8fc\uc5b4\uc9c0\uba70 K1c, \uc989 \ud3c9\uba74 \ubcc0\ud615 \ud30c\uad34\uc778\uc131\uc73c\ub85c \ud45c\uae30\ub41c\ub2e4. \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc870\uac74\uacfc \ub2f4\uae08\uc9c8\uc740 \ub4f1\uae09\uc5d0 \ub530\ub77c \ub2e4\ub974\uba70 \uac01 \ud45c \uc544\ub798\uc758 \ud45c \uc8fc\uc11d\uc5d0 \uae30\uc7ac\ub418\uc5b4 \uc788\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc720\ub0c9 \uacbd\ud654 \ub4f1\uae09(L6 \ubc0f O2)\uc758 \ud30c\uad34\uc778\uc131<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2e8\uc870 \uc555\ud558\uc728, \ub2e8\uba74 \ud06c\uae30, \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uacbd\ub3c4\uc5d0 \ub530\ub978 K1c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uc870 \uc555\ud558\uc728<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \ud06c\uae30<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c (MPa&radic;m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 K1c<\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.86, 18.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.19, 22.14<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">171 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.11, 25.39<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.76, 24.79<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.04, 24.86<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">171 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.53, 28.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.15, 26.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.71, 27.42<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">171 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.12, 30.32<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.37, 17.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.31, 19.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.80, 19.84<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.82, 18.94<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.23, 20.72<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.62, 21.49<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.66, 18.37<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.77, 19.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.31, 20.32<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c II, \uae08\ud615 \ubc0f \ub2e4\uc774\uc6a9 \uacf5\uad6c \uc7ac\ub8cc\uc758 AISI L6 \ubc0f O2 \ud30c\uad34 \uc778\uc131 \uc2dc\ud5d8 \uacb0\uacfc (G. Krauss \ubc0f H. Nordberg \ud3b8).<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ub2e8\uc870 \uc555\ud558\uc728\uc740 432 mm \uc789\uacf3\uc73c\ub85c\ubd80\ud130\uc758 \ucd1d \uc555\ud558\uc728\uc774\ub2e4. L6\ub294 830 &#176;C\uc5d0\uc11c 5\ubd84\uac04 \uc5fc\uc695 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ud6c4 \uc720\ub0c9\ud558\uc600\uace0, O2\ub294 802 &#176;C\uc5d0\uc11c 5\ubd84\uac04 \uc5fc\uc695 \ucc98\ub9ac \ud6c4 \uc720\ub0c9\ud558\uc600\ub2e4. \uac01 \ud589\uc758 \ub450 \uac12\uc740 \ubcc4\ub3c4 \uc2dc\ud3b8\uc5d0 \ub300\ud55c \uac1c\ubcc4 \uc2dc\ud5d8 \uacb0\uacfc\uc774\uba70 \ud3c9\uade0 \uc5f4\uc740 \uc774\ub4e4\uc758 \uc0b0\uc220 \ud3c9\uade0\uc774\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">D3 \ubc0f A6\uc758 \ud30c\uad34\uc778\uc131<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">\uc2dc\ud3b8\uc5d0 \uc608\ube44\uade0\uc5f4\uc744 \ub3c4\uc785\ud558\uc5ec \uc2dc\ud5d8\ud560 \uc218 \uc788\uc5c8\ub358 \uacbd\uc6b0\uc758 K1c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uc870 \uc555\ud558\uc728<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \ud06c\uae30<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c (MPa&radic;m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 K1c<\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">D3<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.54, 33.67<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D3<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.76<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">55.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.81, 21.53<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.63, 21.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">173 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.34, 25.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.95, 20.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.63, 21.77<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">173 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.95, 23.17<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">52.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.41, 27.09<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">49.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.60, 29.46<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">49.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">173 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.06, 29.05<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">48.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c III, \uae08\ud615 \ubc0f \ub2e4\uc774\uc6a9 \uacf5\uad6c \uc7ac\ub8cc\uc758 AISI D3 \ubc0f A6 \ud30c\uad34 \uc778\uc131 \uc2dc\ud5d8 \uacb0\uacfc.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>D3\ub294 \uc2dc\ud5d8\ub41c 9\uac00\uc9c0 \uc870\uac74 \uc911 7\uac00\uc9c0\uc5d0\uc11c \uc608\ube44\uade0\uc5f4 \ub3c4\uc785 \uc911 \uade0\uc5f4\uc774 \ubc1c\uc0dd\ud558\uc600\uc73c\ubbc0\ub85c \ud45c\uc5d0 \uc788\ub294 \ub450 \uac00\uc9c0 \uc870\uac74\ub9cc \uc720\ud6a8\ud55c \uac12\uc744 \uc0b0\ucd9c\ud558\uc600\uace0 \ucd9c\ucc98\ub294 \ub098\uba38\uc9c0\uc5d0 \ub300\ud55c \uc218\uce58\ub97c \uc81c\uacf5\ud558\uc9c0 \uc54a\ub294\ub2e4. D3\ub294 968 &#176;C\uc5d0\uc11c 25\ubd84\uac04 \uc5fc\uc695 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ud6c4 \uc720\ub0c9\ud558\uc600\uace0, A6\ub294 843 &#176;C\uc5d0\uc11c 25\ubd84\uac04 \uc5fc\uc695 \ucc98\ub9ac \ud6c4 \uacf5\ub0c9\ud558\uc600\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uacf5\ub0c9 \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5 \ub4f1\uae09(A2 \ubc0f D2)\uc758 \ud30c\uad34\uc778\uc131<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2e8\uc870 \uc555\ud558\uc728, \ub2e8\uba74 \ud06c\uae30, \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uacbd\ub3c4\uc5d0 \ub530\ub978 K1c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uc870 \uc555\ud558\uc728<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \ud06c\uae30<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c (MPa&radic;m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 K1c<\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.05, 20.69<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.58, 20.78<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.80, 20.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.08, 22.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.58, 21.46<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.40, 21.52<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.31, 22.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.41, 21.96<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.74, 22.09<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.84, 28.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">36.77, 36.58<\/td><td class=\"has-text-align-left\" data-align=\"left\">36.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">167 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">45.35, 40.08, 41.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">42.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">167 mm \uc6d0\ud615, \ud6a1\ubc29\ud5a5<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.07, 30.62<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">38.63, 38.83<\/td><td class=\"has-text-align-left\" data-align=\"left\">38.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">167 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">44.18, 46.32<\/td><td class=\"has-text-align-left\" data-align=\"left\">45.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.85, 25.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.71, 29.87<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">167 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.12, 32.62<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.5<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c IV, \uae08\ud615 \ubc0f \ub2e4\uc774\uc6a9 \uacf5\uad6c \uc7ac\ub8cc\uc758 AISI A2 \ubc0f D2 \ud30c\uad34 \uc778\uc131 \uc2dc\ud5d8 \uacb0\uacfc.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>A2\ub294 954 &#176;C\uc5d0\uc11c 25\ubd84\uac04 \uc5fc\uc695 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ud6c4 \uacf5\ub0c9\ud558\uc600\uace0, D2\ub294 1010 &#176;C\uc5d0\uc11c 25\ubd84\uac04 \uc5fc\uc695 \ucc98\ub9ac \ud6c4 \uacf5\ub0c9\ud558\uc600\ub2e4. 204 &#176;C\uc5d0\uc11c \ud15c\ud37c\ub9c1\ub41c 88 \ud37c\uc13c\ud2b8 \ud589\uc5d0 \ud6a1\ubc29\ud5a5\uc73c\ub85c \ud45c\uc2dc\ub41c \uac83\uc740 167 mm \uc6d0\ud615 \ubd09\uc744 \ub530\ub77c\uac00 \uc544\ub2c8\ub77c \uac00\ub85c\uc9c8\ub7ec \uc808\ub2e8\ud55c \ub2e8\uc77c \uc2dc\ud3b8\uc774\uba70, \ud45c\uc5d0\uc11c \uc720\uc77c\ud55c \ud6a1\ubc29\ud5a5 \ud310\ub3c5\uac12\uc774\ubbc0\ub85c \ubcc4\ub3c4\ub85c \uae30\uc7ac\ub418\uc5c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc5f4\uac04 \uac00\uacf5 \ubc0f \ub0b4\ucda9\uaca9 \ub4f1\uae09(H13 \ubc0f S7)\uc758 \ud30c\uad34\uc778\uc131<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2e8\uc870 \uc555\ud558\uc728, \ub2e8\uba74 \ud06c\uae30, \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uacbd\ub3c4\uc5d0 \ub530\ub978 K1c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uc870 \uc555\ud558\uc728<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \ud06c\uae30<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c (MPa&radic;m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud3c9\uade0 K1c<\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.76, 29.89, 29.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.19, 27.92, 28.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.63, 26.98, 27.54<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">593 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">41.25, 37.50, 38.71<\/td><td class=\"has-text-align-left\" data-align=\"left\">39.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">48.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">593 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.42, 32.74, 31.98<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">47.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">593 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.90, 38.24<\/td><td class=\"has-text-align-left\" data-align=\"left\">37.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">47.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">621 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">87.84, 88.85, 87.74<\/td><td class=\"has-text-align-left\" data-align=\"left\">88.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">621 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">55.02, 80.62, 77.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">71.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">621 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.96, 60.61<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.67, 34.41<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.02, 35.97<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.99, 33.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">38.90, 38.41<\/td><td class=\"has-text-align-left\" data-align=\"left\">38.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">39.48, 39.27<\/td><td class=\"has-text-align-left\" data-align=\"left\">39.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">52.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.28, 35.13<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">51.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.48, 40.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">51.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm \uc815\uc0ac\uac01\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.39, 42.93<\/td><td class=\"has-text-align-left\" data-align=\"left\">41.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">51.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm \uc6d0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.21, 33.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">50.5<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c V, \uae08\ud615 \ubc0f \ub2e4\uc774\uc6a9 \uacf5\uad6c \uc7ac\ub8cc\uc758 AISI H13 \ubc0f S7 \ud30c\uad34 \uc778\uc131 \uc2dc\ud5d8 \uacb0\uacfc.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>H13\uc740 1024 &#176;C \uc5fc\uc695\uc5d0\uc11c 25\ubd84\uac04 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ud6c4 \uacf5\ub7ad\ud588\uace0, S7\uc740 941 &#176;C \uc5fc\uc695\uc5d0\uc11c 25\ubd84\uac04 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ud6c4 \uacf5\ub7ad\ud588\uc2b5\ub2c8\ub2e4. H13 \ud589\uc740 \uac01 \uc628\ub3c4\uc5d0\uc11c 2\uc2dc\uac04\uc529 2\ud68c \ud15c\ud37c\ub9c1\ud588\uc73c\uba70, \uc774\ub294 2\ucc28 \uacbd\ud654 \ud53c\ud06c \ub54c\ubb38\uc5d0 \ub370\uc774\ud130\uc2dc\ud2b8\uc5d0\uc11c \uc694\uad6c\ud558\ub294 \ubc29\uc2dd\uc785\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc5ec\ub35f \uac00\uc9c0 \uac15\uc885\uc744 \ub098\ub780\ud788 \ube44\uad50\ud55c \uacb0\uacfc<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc77c\ubc18\uc801\uc778 \uc791\uc5c5 \uacbd\ub3c4\uc5d0\uc11c \uc774 \uac15\uc885\ub4e4\uc740 \uacf5\uad6c \uc5c5\uacc4\uac00 \uc774\ubbf8 \uc0ac\uc6a9\ud558\ub294 \uc138 \uadf8\ub8f9\uc73c\ub85c \ub098\ub258\uba70, \ud45c\ub294 \uadf8 \uad6c\ubd84\uc5d0 \uc218\uce58\ub97c \ubd80\uc5ec\ud569\ub2c8\ub2e4. \uc720\ub0c9 \uacbd\ud654\ud615 L6\uc740 \uc5ec\ub35f \uac00\uc9c0 \uc911 \uc778\uc131\uc774 \uac00\uc7a5 \ub192\uc544 60 HRC\uc5d0\uc11c 19.7 MPa root metre\ubd80\ud130 53.5 HRC\uc5d0\uc11c 29.7\uae4c\uc9c0\uc785\ub2c8\ub2e4. O2\ub294 \uac19\uc740 \uacbd\ub3c4 \ubc94\uc704\uc5d0\uc11c 17.9~20.3\uc73c\ub85c \uadf8 \uc544\ub798\uc5d0 \uc704\uce58\ud569\ub2c8\ub2e4. \ub0b4\ub9c8\ubaa8\uc131 \ud06c\ub86c \uac15\uc885\uc774 \uadf8\ub2e4\uc74c\uc73c\ub85c, D3\ub294 32.8~33.7, D2\ub294 \ub2e8\uba74\uacfc \ud15c\ud37c\ub9c1\uc5d0 \ub530\ub77c 25.2~45.2\uc778 \ubc18\uba74, A2\ub294 \uc804 \ubc94\uc704\uc5d0\uc11c 20.9~22.3\uc758 \uc881\uc740 \ud3ed\uc744 \uc720\uc9c0\ud569\ub2c8\ub2e4. \uc5f4\uac04 \ubc0f \ucda9\uaca9\uc6a9 \uac15\uc885\uc774 \uac00\uc7a5 \ub192\uc544, S7\uc740 57 HRC\uc5d0\uc11c 34.5\uc5d0 \ub3c4\ub2ec\ud558\uace0 H13\uc740 53.5\uc5d0\uc11c 40.0 HRC\ub85c \ud15c\ud37c\ub9c1\ub428\uc5d0 \ub530\ub77c 27.4~88.0\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud45c\uc5d0\uc11c \ub450 \uac00\uc9c0 \ud310\ub3c5\uac12\uc740 \uc77c\ubc18\uc801\uc778 \uacbd\ud5d8 \ubc95\uce59\uc5d0 \uc5b4\uae0b\ub098\ubbc0\ub85c \uc8fc\ubaa9\ud560 \ub9cc\ud569\ub2c8\ub2e4. D2\ub294 \uc5c5\uacc4\uc5d0\uc11c \ud1b5\uc0c1 \uc778\uc815\ud558\ub294 \uac83\ubcf4\ub2e4 \ub192\uc740 \ud30c\uad34\uc778\uc131\uc744 \ubcf4\uc600\uc73c\uba70 H13\uacfc \uac19\uc740 \uc601\uc5ed\uc5d0 \uc788\uace0, 204 &#176;C\uc5d0\uc11c\uc758 88\ud37c\uc13c\ud2b8 \ud589\uc740 42.1 MPa root metre\uc5d0 \ub3c4\ub2ec\ud588\uc2b5\ub2c8\ub2e4. \ub2e4\ub978 \ud558\ub098\ub294 \uac19\uc740 D2 \ubd09\uc7ac\uc5d0\uc11c \uc885\ubc29\ud5a5\uacfc \ud6a1\ubc29\ud5a5\uc758 \ucc28\uc774\ub85c, 42.1 \ub300 25.0\uc785\ub2c8\ub2e4. \ud6a1\ubc29\ud5a5 \ud310\ub3c5\uac12\uc740 \uc885\ubc29\ud5a5\ubcf4\ub2e4 \uc644\uc131\ub41c \ub2e4\uc774\uc5d0 \ub300\ud574 \ub354 \ub9ce\uc740 \uac83\uc744 \uc54c\ub824\uc8fc\ub294\ub370, \uacf5\uad6c\ub294 \ubcf4\ud1b5 \ubd09\uc7ac\uac00 \uac00\uacf5\ub41c \ubc29\ud5a5\uc744 \uac00\ub85c\uc9c8\ub7ec \ud30c\uc190\ub418\ubbc0\ub85c \uc885\ubc29\ud5a5 \uc778\uc131\ub9cc\uc73c\ub85c \uc791\uc131\ub41c \uc0ac\uc591\uc740 \uac15\uc885\uc744 \uc2e4\uc81c\ubcf4\ub2e4 \uc88b\uac8c \ubcf4\uc774\uac8c \ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uacbd\ub3c4 \uc5f4\uc744 \uc778\uc131\uacfc \ub300\uc870\ud574 \uc77d\uc73c\uba74 \uc77c\ubc18 \uc791\uc5c5 \uacbd\ub3c4 \uc774\ud558\ub85c \ud15c\ud37c\ub9c1\ud558\ub294 \uac83\uc774 \uc548\uc804\uc744 \ud655\ubcf4\ud558\ub294 \ubc29\ubc95\uc774 \uc544\ub2cc \uc774\uc720\ub3c4 \ub4dc\ub7ec\ub0a9\ub2c8\ub2e4. L6, O2, A2, A6 \ud589\uc5d0\uc11c \ud3c9\uade0 \uc778\uc131\uc740 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uac00 \uc62c\ub77c\uac00\uace0 \uacbd\ub3c4\uac00 \ub0b4\ub824\uac10\uc5d0 \ub530\ub77c \uc0c1\uc2b9\ud558\uba70, \uadf8 \uc0c1\uc2b9\uc740 \uae09\uaca9\ud558\uc9c0 \uc54a\uace0 \uafb8\uc900\ud569\ub2c8\ub2e4. \uc778\uc131\uc744 \uc5bb\uae30 \uc704\ud574 \uac15\uc885\uc744 \ub354 \ub0ae\uc740 \uacbd\ub3c4\ub85c \uac15\uc81c\ud558\ub294 \uac83\uc740 \ub0b4\ub9c8\ubaa8\uc131\ub3c4 \ud76c\uc0dd\uc2dc\ud0a4\uba70, \uc5bb\ub294 \uc778\uc131 \uc99d\uac00\ub294 \uac15\uc885\uc744 \ubc14\uafc0 \ub54c\uc758 \uc0c1\uc2b9\ud3ed\ubcf4\ub2e4 \uc791\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc218\uce58\ub294 \uacf5\uac1c\ub41c \uc2e4\ud5d8\uac12\uc774\uba70 \ucc38\uace0 \uc694\uc57d\uc77c \ubfd0\uc785\ub2c8\ub2e4. \ud30c\uad34\uc778\uc131\uc740 \uc2dc\ud3b8 \ubc29\ud5a5, \ub2e8\uba74 \ud06c\uae30, \uc5f4\ucc98\ub9ac\uc5d0 \ubbfc\uac10\ud558\ubbc0\ub85c \ud45c\ub97c \ud2b9\uc815 \ubd80\ud488\uc758 \uc124\uacc4\uac12\uc774 \uc544\ub2c8\ub77c \uac15\uc885 \uac04 \ube44\uad50\ub85c \ucde8\uae09\ud558\uc2ed\uc2dc\uc624. \uc7ac\ub8cc \uc2dc\ud5d8 \uc131\uc801\uc11c\ub85c \ud655\uc778\ud558\uac70\ub098 Aobo Steel\uc5d0 \ubb38\uc758\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ub370\uc774\ud130<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uac19\uc740 \uc8fc\uc81c\uc758 \ucda9\uaca9 \uce21\uba74\uc740 \ub3d9\uc77c \ud504\ub85c\uadf8\ub7a8\uc758 \ubb34\ub178\uce58 Izod \ubc0f Charpy V-\ub178\uce58 \uc2dc\ud3b8\uc73c\ub85c \uce21\uc815\ud588\uc73c\uba70, \uc800\ud76c <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-impact-toughness-chart\/\">\uacf5\uad6c\uac15 \ucda9\uaca9 \uc778\uc131 \ucc28\ud2b8<\/a>\uc5d0 \uc788\uc2b5\ub2c8\ub2e4. \uc774 \uc778\uc131 \uc218\uce58\ub97c \uac15\uc885 \uc120\ud0dd\uc73c\ub85c \uc804\ud658\ud558\ub294 \ub2e4\uc774 \uc120\uc815\uc5d0 \ub300\ud574\uc11c\ub294 \ub2e4\uc74c \ud398\uc774\uc9c0\ub97c \ucc38\uc870\ud558\uc2ed\uc2dc\uc624: <a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel\/\">D2 \uacf5\uad6c\uac15<\/a>, <a href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel\/\">H13 \uacf5\uad6c\uac15<\/a>, <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel\/\">A2 \uacf5\uad6c\uac15<\/a> \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/s7-tool-steel\/\">S7 \uacf5\uad6c\uac15<\/a>, \uadf8\ub9ac\uace0 \ub2e4\uc74c \uac00\uc774\ub4dc: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steels-for-chipping-resistance\/\">\uce58\ud551 \uc800\ud56d\uc131 \uacf5\uad6c\uac15<\/a> \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steels-for-cracking-resistance\/\">\uade0\uc5f4 \uc800\ud56d\uc131\uc744 \uc704\ud55c \uacf5\uad6c\uac15<\/a>.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uacf5\uad6c\uac15 \ud30c\uad34\uc778\uc131 \ucc28\ud2b8, \uc778\uc1c4\uc6a9 PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uc704\uc758 \ub124 \uac00\uc9c0 K1c \ud45c\ub97c L6\uc640 O2\ubd80\ud130 D3, A6, A2, D2, H13, S7\uae4c\uc9c0 \ud558\ub098\uc758 PDF\ub85c \uc815\ub9ac\ud588\uc73c\uba70, \ub2f9\uc0ac \uc5f0\ub77d\ucc98 \uc815\ubcf4\ub3c4 \ud3ec\ud568\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fracture-Toughness-Chart.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 533 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: \uae08\ud615 \ubc0f \ub2e4\uc774\uc6a9 \uacf5\uad6c \uc7ac\ub8cc, \uc751\uc6a9 \ubc0f \uc131\ub2a5 (G. Krauss \ubc0f H. Nordberg \ud3b8\uc9d1).<\/p>","protected":false},"excerpt":{"rendered":"<p>Tool Steel Fracture Toughness Chart (K1c) Fracture toughness in MPa root metre for eight common tool steel grades, measured on bend bars taken from three forging reductions and tempered at three temperatures, with the hardness each specimen was tested at. A reference summary of published practice and not an Aobo Steel specification. How the values [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20442","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Tool Steel Fracture Toughness Chart (K1c) | Aobo Steel<\/title>\n<meta name=\"description\" content=\"Fracture toughness (K1c) of L6, O2, D3, A6, A2, D2, H13 and S7 tool steels by forging reduction, section size, tempering temperature and hardness.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/tool-steel-fracture-toughness-chart\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Tool Steel Fracture Toughness Chart (K1c)\" \/>\n<meta property=\"og:description\" content=\"Fracture toughness (K1c) of L6, O2, D3, A6, A2, D2, H13 and S7 tool steels by forging reduction, section size, tempering temperature and hardness.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/tool-steel-fracture-toughness-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:40:35+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"8\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Tool Steel Fracture Toughness Chart (K1c)\",\"datePublished\":\"2026-10-01T01:11:55+00:00\",\"dateModified\":\"2026-10-15T16:40:35+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\"},\"wordCount\":1538,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\",\"name\":\"Tool Steel Fracture Toughness Chart (K1c) | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-01T01:11:55+00:00\",\"dateModified\":\"2026-10-15T16:40:35+00:00\",\"description\":\"Fracture toughness (K1c) of L6, O2, D3, A6, A2, D2, H13 and S7 tool steels by forging reduction, section size, tempering temperature and hardness.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Tool Steel Fracture Toughness Chart (K1c)\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uacf5\uad6c\uac15 \ud30c\uad34\uc778\uc131\ud45c (K1c) | Aobo Steel","description":"L6, O2, D3, A6, A2, D2, H13, S7 \uacf5\uad6c\uac15\uc758 \ud30c\uad34\uc778\uc131(K1c)\uc744 \ub2e8\uc870 \uc555\ud558\uc728, \ub2e8\uba74 \ud06c\uae30, \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uacbd\ub3c4\ubcc4\ub85c \uc81c\uc2dc\ud569\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/tool-steel-fracture-toughness-chart\/","og_locale":"ko_KR","og_type":"article","og_title":"Tool Steel Fracture Toughness Chart (K1c)","og_description":"Fracture toughness (K1c) of L6, O2, D3, A6, A2, D2, H13 and S7 tool steels by forging reduction, section size, tempering temperature and hardness.","og_url":"https:\/\/aobosteel.com\/ko\/tool-steel-fracture-toughness-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:40:35+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"8\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Tool Steel Fracture Toughness Chart (K1c)","datePublished":"2026-10-01T01:11:55+00:00","dateModified":"2026-10-15T16:40:35+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/"},"wordCount":1538,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/","url":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/","name":"\uacf5\uad6c\uac15 \ud30c\uad34\uc778\uc131\ud45c (K1c) | Aobo Steel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-01T01:11:55+00:00","dateModified":"2026-10-15T16:40:35+00:00","description":"L6, O2, D3, A6, A2, D2, H13, S7 \uacf5\uad6c\uac15\uc758 \ud30c\uad34\uc778\uc131(K1c)\uc744 \ub2e8\uc870 \uc555\ud558\uc728, \ub2e8\uba74 \ud06c\uae30, \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uacbd\ub3c4\ubcc4\ub85c \uc81c\uc2dc\ud569\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Tool Steel Fracture Toughness Chart (K1c)"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tool Steel Fracture Toughness Chart (K1c) Fracture toughness in MPa root metre for eight common tool steel grades, measured on bend bars taken from three forging reductions and tempered at three temperatures, with the hardness each specimen was tested at. A reference summary of published practice and not an Aobo Steel specification. How the values&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tool Steel Fracture Toughness Chart (K1c) Fracture toughness in MPa root metre for eight common tool steel grades, measured on bend bars taken from three forging reductions and tempered at three temperatures, with the hardness each specimen was tested at. A reference summary of published practice and not an Aobo Steel specification. How the values&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20442","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20442"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20442\/revisions"}],"predecessor-version":[{"id":22542,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20442\/revisions\/22542"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20442"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}