{"id":20425,"date":"2026-10-01T06:06:40","date_gmt":"2026-09-30T22:06:40","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20425"},"modified":"2026-10-16T00:38:39","modified_gmt":"2026-10-15T16:38:39","slug":"tool-steel-heat-treatment-temperature-ranges","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-temperature-ranges\/","title":{"rendered":"\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uc628\ub3c4 \ubc94\uc704 \ubc0f \uae30\uc900\uc810"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uc628\ub3c4 \ubc94\uc704 \ubc0f \uae30\uc900\uc810<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\uacf5\uad6c \ubc0f \uae08\ud615 \uc81c\uc791 \ud578\ub4dc\ubd81\uc5d0\uc11c \ubc1c\ucdcc\ud55c, \uacf5\uad6c\uac15\uc758 \uacbd\ud654, \uc5b4\ub2d0\ub9c1, \uce68\ud0c4, \uc9c8\ud654 \ubc0f \uc751\ub825 \uc81c\uac70 \uc628\ub3c4 \ubc94\uc704\uc640 \uadf8 \uc704\uc758 \uc5f4\uc6d0 \ubc0f \uc544\ub798\uc758 \uc11c\ube0c\uc81c\ub85c \ubc94\uc704\uc785\ub2c8\ub2e4. \uacf5\uac1c\ub41c \uc2e4\ubb34 \uad00\ud589\uc744 \uc694\uc57d\ud55c \ucc38\uace0 \uc790\ub8cc\uc774\uba70 Aobo Steel\uc758 \uc0ac\uc591\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud45c \uc77d\ub294 \ubc29\ubc95<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ub2e4\uc74c\uc740 \uacf5\uad6c \ubc0f \uae08\ud615 \uc791\uc5c5 \uc804\ubc18\uc5d0\uc11c \ub4f1\uc7a5\ud558\ub294 \uc628\ub3c4\ub4e4\uc744 \ud55c\uacf3\uc5d0 \ubaa8\uc740 \uac83\uc73c\ub85c, \uacbd\ud654, \uc5b4\ub2d0\ub9c1 \ubc0f \ud45c\uba74 \ucc98\ub9ac \ubc94\uc704\ub97c \uc774\ub97c \ubc1c\uc0dd\uc2dc\ud0a4\ub294 \uc5f4\uc6d0\uacfc \uce21\uc815 \uae30\uc900\uc774 \ub418\ub294 \uc800\uc628 \ub05d\ub2e8\uc5d0 \ub300\ube44\ud558\uc5ec \uc77d\uc744 \uc218 \uc788\ub3c4\ub85d \ud55c \uac83\uc785\ub2c8\ub2e4. \ubaa8\ub4e0 \uc218\uce58\ub294 \ud654\uc528\ub85c \ud45c\uae30\ub418\uc5b4 \uc788\uc73c\uba70 \ucc45 \uc790\uccb4\uc758 \uc12d\uc528 \ud658\uc0b0\uac12\uc774 \uc606\uc5d0 \ud568\uaed8 \uc778\uc1c4\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. \uc774\ub294 \ub2e8\uc77c \uc5f4\ucc98\ub9ac \uc124\uc815\uc774 \uc544\ub2c8\ub77c \uc5ec\ub7ec \uac15\uc885 \uadf8\ub8f9\uc5d0 \ub300\ud55c \ubc94\uc704\uc774\uba70, \ud2b9\uc815 \uac15\uc885\uc774 \ubc94\uc704 \ub0b4 \uc5b4\ub514\uc5d0 \uc704\uce58\ud558\ub294\uc9c0\ub294 \ud569\uae08 \uc131\ubd84\uacfc \ucc98\ub9ac\ub418\ub294 \ub2e8\uba74\uc5d0 \uc758\ud574 \uacb0\uc815\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2e4\uc591\ud55c \uc791\uc5c5 \ubc0f \uc870\uac74\uc5d0 \ub300\ud55c \uc628\ub3c4<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc791\uc5c5 \ub610\ub294 \uc870\uac74<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0C<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud145\uc2a4\ud150 \uc544\ud06c<\/td><td class=\"has-text-align-left\" data-align=\"left\">11,600<\/td><td class=\"has-text-align-left\" data-align=\"left\">(6,427)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ucca0 \uc6a9\uc811 \uc544\ud06c<\/td><td class=\"has-text-align-left\" data-align=\"left\">10,800<\/td><td class=\"has-text-align-left\" data-align=\"left\">(5,982)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc0b0\uc18c\uc544\uc138\ud2f8\ub80c \ud654\uc5fc<\/td><td class=\"has-text-align-left\" data-align=\"left\">6,300<\/td><td class=\"has-text-align-left\" data-align=\"left\">(3,482)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">MAPP \uac00\uc2a4<\/td><td class=\"has-text-align-left\" data-align=\"left\">5,301<\/td><td class=\"has-text-align-left\" data-align=\"left\">(2,927)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud504\ub85c\ud310 \ud654\uc5fc<\/td><td class=\"has-text-align-left\" data-align=\"left\">5,300<\/td><td class=\"has-text-align-left\" data-align=\"left\">(2,927)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc0b0\uc18c\uc218\uc18c<\/td><td class=\"has-text-align-left\" data-align=\"left\">5,072<\/td><td class=\"has-text-align-left\" data-align=\"left\">(2,800)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc2e4\ud5d8\uc2e4 \ubc84\ub108<\/td><td class=\"has-text-align-left\" data-align=\"left\">3,360<\/td><td class=\"has-text-align-left\" data-align=\"left\">(1,849)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ucca0 \uc6a9\uc735 (\uc561\uccb4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2,800<\/td><td class=\"has-text-align-left\" data-align=\"left\">(1,538)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc6a9\uc811 \ubc0f \uac15 \uc6a9\uc735<\/td><td class=\"has-text-align-left\" data-align=\"left\">2,400<\/td><td class=\"has-text-align-left\" data-align=\"left\">(1,316)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uace0\uc18d\ub3c4\uac15 \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">2,100\u20132,400<\/td><td class=\"has-text-align-left\" data-align=\"left\">(1,149\u20131,316)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud569\uae08 \uacf5\uad6c\uac15 \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">1,500\u20131,900<\/td><td class=\"has-text-align-left\" data-align=\"left\">(816\u20131,038)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uce68\ud0c4 \ubc94\uc704<\/td><td class=\"has-text-align-left\" data-align=\"left\">1,700\u20131,800<\/td><td class=\"has-text-align-left\" data-align=\"left\">(927\u2013982)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud654\uc5fc \uacbd\ud654 \ubc94\uc704 (4140 \/ 4150)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1,550\u20131,600<\/td><td class=\"has-text-align-left\" data-align=\"left\">(843\u2013871)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1 \ubc94\uc704<\/td><td class=\"has-text-align-left\" data-align=\"left\">1,400\u20131,700<\/td><td class=\"has-text-align-left\" data-align=\"left\">(760\u2013927)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud0c4\uc18c\uac15 \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">1,350\u20131,550<\/td><td class=\"has-text-align-left\" data-align=\"left\">(732\u2013843)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc2a4\ud2b8\ub808\uc2a4 \ud574\uc18c<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u20131,200<\/td><td class=\"has-text-align-left\" data-align=\"left\">(204\u2013649)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc9c8\ud654 \ubc94\uc704<\/td><td class=\"has-text-align-left\" data-align=\"left\">900\u20131,000<\/td><td class=\"has-text-align-left\" data-align=\"left\">(482\u2013538)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uccad\uc5f4 \ucde8\uc131 \ubc94\uc704<\/td><td class=\"has-text-align-left\" data-align=\"left\">600\u2013800<\/td><td class=\"has-text-align-left\" data-align=\"left\">(316\u2013427)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubb3c \ube44\ub4f1<\/td><td class=\"has-text-align-left\" data-align=\"left\">212<\/td><td class=\"has-text-align-left\" data-align=\"left\">(100)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5bc\uc74c \uc735\ud574<\/td><td class=\"has-text-align-left\" data-align=\"left\">32<\/td><td class=\"has-text-align-left\" data-align=\"left\">(0)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud654\uc528 \uc601\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">(-18)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub4dc\ub77c\uc774\uc544\uc774\uc2a4<\/td><td class=\"has-text-align-left\" data-align=\"left\">-120<\/td><td class=\"has-text-align-left\" data-align=\"left\">(-84)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc601\ud558\uc758 \ucc98\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">-320 to 0<\/td><td class=\"has-text-align-left\" data-align=\"left\">(-196 to -18)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc808\ub300 \uc601\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">-460<\/td><td class=\"has-text-align-left\" data-align=\"left\">(-273)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud45c 8-1, Tool and Die Making Troubleshooter (Richard M. Leed)\uc758 \ub2e4\uc591\ud55c \uc791\uc5c5 \ubc0f \uc870\uac74\uc5d0 \ub300\ud55c \uc628\ub3c4. \uc774 \ucc45\uc740 Bethlehem Steel Corp., 1936\uc744 \uc778\uc6a9\ud568.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ud45c\uc758 MAPP \uac00\uc2a4\ub294 \ucc45\uc5d0\uc11c \uba85\uc2dc\ud55c \uc561\ud654\uc11d\uc720 \ubc0f \uba54\ud2f8\uc544\uc138\ud2f8\ub80c-\ud504\ub85c\ud30c\ub514\uc5d4 \ud63c\ud569\ubb3c\uc774\uba70, \ud654\uc5fc \uacbd\ud654 \ubc94\uc704\ub294 4140 \ubc0f 4150\uc5d0 \ub300\ud574 \uae30\uc7ac\ub418\uc5b4 \uc788\ub294\ub370, \uc774\ub294 \uacf5\uad6c\uac15\uc774 \uc544\ub2cc \uae30\uc900\uc810\uc73c\ub85c \uc778\uc1c4\ub41c \uac83\uc785\ub2c8\ub2e4. \uc12d\uc528 \uc628\ub3c4\ub294 \ucc45 \uc790\uccb4\uc758 \ud658\uc0b0\uac12\uc73c\ub85c, \ucd9c\ucc98\uc5d0 \uc778\uc1c4\ub41c \uadf8\ub300\ub85c \uad04\ud638 \uc548\uc5d0 \ud45c\uc2dc\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \ubc94\uc704\uc758 \uc704\uce58<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uacf5\uad6c\uac15 \uad6c\ub9e4\uc790\uac00 \uc77c\ubc18\uc801\uc73c\ub85c \uc81c\uc2dc\ubc1b\ub294 \ubc94\uc704\ub294 \ud45c\uc758 \uc911\uac04\uc5d0 \uc788\ub294 \uac83\ub4e4\uc785\ub2c8\ub2e4. \ud569\uae08 \uacf5\uad6c\uac15\uc740 1,500~1,900 &deg;F (816~1,038 &deg;C)\uc5d0\uc11c \uacbd\ud654\ub418\uba70, \uace0\uc18d\ub3c4\uac15\uc740 \ud0c4\ud654\ubb3c\uc774 \uace0\uc6a9\ub418\uae30 \uc804\uc5d0 2,100~2,400 &deg;F (1,149~1,316 &deg;C)\uac00 \ud544\uc694\ud569\ub2c8\ub2e4. \uc5b4\ub2d0\ub9c1\uc740 \uacbd\ud654 \ubc94\uc704 \uc544\ub798\uc778 1,400~1,700 &deg;F (760~927 &deg;C), \uce68\ud0c4\uc740 1,700~1,800 &deg;F (927~982 &deg;C), \uc9c8\ud654\ub294 900~1,000 &deg;F (482~538 &deg;C)\uc5d0 \uc704\uce58\ud558\uba70, \uc751\ub825 \uc81c\uac70\ub294 400~1,200 &deg;F (204~649 &deg;C)\uc758 \ub113\uc740 \ubc94\uc704\uc5d0 \uac78\uccd0 \uc788\uc2b5\ub2c8\ub2e4. 600~800 &deg;F (316~427 &deg;C)\uc758 \uccad\uc5f4 \ucde8\uc131 \ubc94\uc704\ub294 \ud15c\ud37c\ub9c1\ub41c \ubd80\ud488\uc774 \ucda9\uaca9 \uc778\uc131\uc744 \uc0c1\uc2e4\ud558\ub294 \uad6c\uac04\uc73c\ub85c, \uc774 \ub54c\ubb38\uc5d0 \ud15c\ud37c\ub9c1\uc740 \uc885\uc885 \uc774 \ubc94\uc704 \uc544\ub798\ub098 \ud6e8\uc52c \uc704\uc5d0\uc11c \uc218\ud589\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774\ub7ec\ud55c \ubc94\uc704 \ub4a4\uc5d0 \uc788\ub294 \uac15\uc885\ubcc4 \uc218\uce58\ub294 \ub2e4\uc74c \ud398\uc774\uc9c0\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-hardening-tempering-chart\/\">\uacf5\uad6c\uac15 \uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1 \ucc28\ud2b8<\/a>, <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-annealing-normalizing-temperature-chart\/\">\uc5b4\ub2d0\ub9c1 \ubc0f \ub178\uba40\ub77c\uc774\uc9d5 \uc628\ub3c4<\/a> \ubc0f <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-guide\/\">\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub3d9\uc77c\ud55c \uc2a4\ucf00\uc904\uc744 \ud0c4\uc18c \ud568\ub7c9\uc5d0 \ub300\ud574 \uadf8\ub824\uc9c4 \ub2e8\uc77c \ub2e4\uc774\uc5b4\uadf8\ub7a8\uc5d0\uc11c \ubcc0\ud0dc\uc120\uacfc \ud568\uaed8 \uc77d\uc744 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg\" alt=\"Heat treatment temperature ranges for carbon and tool steels against carbon content: hot working, normalizing, annealing, quenching, recrystallization and stress relief annealing\"\/><figcaption class=\"wp-element-caption\">\uadf8\ub9bc 11.9. \ud0c4\uc18c \ud568\ub7c9\uc5d0 \ub530\ub978 \ud0c4\uc18c\uac15 \ubc0f \uacf5\uad6c\uac15\uc758 \uc5f4\ucc98\ub9ac \uc628\ub3c4 \ubc94\uc704: \uc5f4\uac04 \uac00\uacf5, \ub178\uba40\ub77c\uc774\uc9d5, \uc5f0\ud654 \uc5b4\ub2d0\ub9c1, \uc218\ub0c9 \ub2f4\uae08\uc9c8, \uc720\ub0c9 \ub2f4\uae08\uc9c8, \uc7ac\uacb0\uc815 \uc5b4\ub2d0\ub9c1 \ubc0f \uc751\ub825 \uc81c\uac70 \uc5b4\ub2d0\ub9c1, A<sub>1<\/sub>, A<sub>3<\/sub> and A<sub>\uc13c\ud2f0\ubbf8\ud130<\/sub> \uc120\uc774 \ud45c\uc2dc\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. \uc774 \ub2e4\uc774\uc5b4\uadf8\ub7a8\uc740 \uc77c\ubc18\uc801\uc778 \uacbd\uc6b0\uc774\uba70, \uac1c\ubcc4 \uac15\uc885\uc758 \ubc94\uc704\ub294 \uc704 \ud45c\uc5d0 \uc788\uace0, \uac15\uc885\ubcc4 \uc2a4\ucf00\uc904\uc740 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc\uc5d0 \uc788\uc2b5\ub2c8\ub2e4. \ucd9c\ucc98: E. Essadiqi, Tool Steels, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 11.9.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">\ubc94\uc704\uac00 \uc801\uc6a9\ub418\ub294 \uac15\uc885<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uace0\uc18d\ub3c4\uac15 \ubc94\uc704\ub294 \ub2e4\uc74c\uc5d0 \ud574\ub2f9\ud569\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/m2-tool-steel\/\">M2 \uacf5\uad6c\uac15<\/a> \ubc0f \uae30\ud0c0 \ubab0\ub9ac\ube0c\ub374 \uace0\uc18d\ub3c4\uac15 \uac15\uc885, \ud569\uae08 \uacf5\uad6c\uac15 \ubc94\uc704\ub294 \ub2e4\uc74c\uacfc \uac19\uc740 \ub0c9\uac04 \uac00\uacf5 \uac15\uc885\uc744 \ud3ec\ud568\ud569\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel\/\">D2 \uacf5\uad6c\uac15<\/a> \ubc0f \uacf5\uae30 \uacbd\ud654 \uacc4\uc5f4, \uadf8\ub9ac\uace0 \ub2e4\uc74c\uacfc \uac19\uc740 \uc5f4\uac04 \uac00\uacf5 \uac15\uc885\uc740 <a href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel\/\">H13 \uacf5\uad6c\uac15<\/a> \ub3d9\uc77c\ud55c \ubc94\uc704 \ub0b4\uc5d0\uc11c \uacbd\ud654\ub41c \ud6c4 \uace0\uc628 \uacbd\ub3c4\ub97c \uc704\ud574 \ud15c\ud37c\ub9c1\ub429\ub2c8\ub2e4. \ud2b9\uc815 \uac15\uc885\uc758 \uacbd\ud654 \uc628\ub3c4\uc640 \uadf8\uc5d0 \ub530\ub978 \uc720\uc9c0 \uc2dc\uac04\uc740 \ub2e4\uc74c \ud398\uc774\uc9c0\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steels\/\">\uacf5\uad6c\uac15 \uce74\ud0c8\ub85c\uadf8<\/a> \ub4f1\uae09 \ud398\uc774\uc9c0.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud45c\uc758 \uc0c1\ub2e8, \uc5f4\uc6d0<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uccab \ubc88\uc9f8 \ud589\ub4e4\uc740 \uc5f4\ucc98\ub9ac\ub85c\uac00 \uc124\uc815\ub418\ub294 \uc628\ub3c4\uac00 \uc544\ub2c8\ub77c \uc5f4\uc6d0\uc774 \ub3c4\ub2ec\ud558\ub294 \uc628\ub3c4\uc785\ub2c8\ub2e4. \ud145\uc2a4\ud150 \uc544\ud06c\ub294 11,600 &deg;F (6,427 &deg;C)\uc5d0\uc11c \uc791\ub3d9\ud558\uace0 \uc0b0\uc18c-\uc544\uc138\ud2f8\ub80c \ubd88\uaf43\uc740 6,300 &deg;F (3,482 &deg;C)\uc5d0\uc11c \uc791\ub3d9\ud558\uba70, \ub458 \ub2e4 \ubaa8\ub4e0 \uacbd\ud654 \ubc94\uc704\ubcf4\ub2e4 \ud6e8\uc52c \ub192\uc2b5\ub2c8\ub2e4. \uc774\uac83\uc774 \ud1a0\uce58\ub098 \uc544\ud06c\uac00 \ubd80\ud488 \uc790\uccb4\uac00 \uc628\ub3c4\uc5d0 \ub3c4\ub2ec\ud558\uae30 \ud6e8\uc52c \uc804\uc5d0 \ub2e4\uc774 \ud45c\uba74\uc744 \uc6a9\uc735\uc2dc\ud0a4\ub294 \uc774\uc720\uc785\ub2c8\ub2e4. \ucca0\uc740 2,800 &deg;F (1,538 &deg;C)\uc5d0\uc11c \uc6a9\uc735\ub418\uba70, \uc774 \uc218\uce58\ub294 \uac15\uc774 \uace0\uccb4\ub85c \uc720\uc9c0\ub418\uc5b4\uc57c \ud558\ub294 \ubaa8\ub4e0 \uc791\uc5c5\uc758 \uc2e4\uc9c8\uc801\uc778 \uc0c1\ud55c\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc800\uc628\ubd80 \ubc0f \uc11c\ube0c\uc81c\ub85c \ucc98\ub9ac<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ub4dc\ub77c\uc774\uc544\uc774\uc2a4\ub294 -120 &deg;F (-84 &deg;C)\uc5d0 \uc704\uce58\ud558\uba70 \uc11c\ube0c\uc81c\ub85c \ucc98\ub9ac\ub294 -320\uc5d0\uc11c 0 &deg;F (-196\uc5d0\uc11c -18 &deg;C)\uae4c\uc9c0 \uc2e4\ud589\ub418\uc5b4, \ub300\uccb4\ub41c \ub4dc\ub77c\uc774\uc544\uc774\uc2a4\ubcf4\ub2e4 \ub0ae\uc2b5\ub2c8\ub2e4. \uc808\ub300 \uc601\ub3c4\uc778 -460 &deg;F (-273 &deg;C)\ub294 \ud45c \ud558\ub2e8\uc5d0 \uc778\uc1c4\ub418\uc5b4 \uc788\ub294\ub370, \uc774\ub294 \uc791\uc5c5\uc7a5\uc5d0\uc11c \uc791\uc5c5\ud558\ub294 \uc628\ub3c4\uac00 \uc544\ub2c8\ub77c \ub208\uae08\uc774 \uad6c\ucd95\ub41c \ubc14\ub2e5\uc774\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uacf5\uad6c\uac15 \uc0ac\uc774\ud074\uc758 \uc11c\ube0c\uc81c\ub85c \ub2e8\uacc4\ub294 \ub2f4\uae08\uc9c8\uc774 \uc911\ub2e8\uc2dc\ud0a8 \ubcc0\ud0dc\ub97c \uacc4\uc18d\ud558\uba70, \uc800\ud76c \ud398\uc774\uc9c0\uc5d0\uc11c\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/cryogenic-treatment-of-tool-steel\/\">\uacf5\uad6c\uac15\uc758 \uadf9\uc800\uc628 \ucc98\ub9ac<\/a> \uc5b8\uc81c \uc0ac\uc6a9\ub418\ub294\uc9c0\uc640 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc5d0 \ubbf8\uce58\ub294 \uc601\ud5a5\uc744 \ub2e4\ub8f9\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uc628\ub3c4 \ubc94\uc704, \uc778\uc1c4 \uac00\ub2a5\ud55c PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uc704\uc758 \uc628\ub3c4 \ud45c\ub97c \uc800\ud76c \uc5f0\ub77d\ucc98 \uc815\ubcf4\uc640 \ud568\uaed8 \ud55c \uc7a5\uc5d0 \ub2f4\uc544 \uc791\uc5c5\uc7a5 \ubcbd\uc5d0 \ubd99\uc77c \uc218 \uc788\ub3c4\ub85d \ud588\uc2b5\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Heat-Treatment-Temperature-Ranges.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 382 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: Tool and Die Making Troubleshooter (Richard M. Leed).<\/p>","protected":false},"excerpt":{"rendered":"<p>Tool Steel Heat Treatment Temperature Ranges and Reference Points The temperature ranges tool steel is hardened, annealed, carburized, nitrided and stress relieved at, with the heat sources above them and the subzero range below, from a tool and die shop handbook. A reference summary of published practice and not an Aobo Steel specification. How to [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20425","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Tool Steel Heat Treatment Temperature Ranges | Aobo Steel<\/title>\n<meta name=\"description\" content=\"The hardening, annealing, carburizing, nitriding and stress relieving ranges for tool steel, with the heat sources above them and the subzero range below, from a tool and die handbook.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-temperature-ranges\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Tool Steel Heat Treatment Temperature Ranges and Reference Points\" \/>\n<meta property=\"og:description\" content=\"The hardening, annealing, carburizing, nitriding and stress relieving ranges for tool steel, with the heat sources above them and the subzero range below, from a tool and die handbook.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-temperature-ranges\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:38:39+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"5\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Tool Steel Heat Treatment Temperature Ranges and Reference Points\",\"datePublished\":\"2026-09-30T22:06:40+00:00\",\"dateModified\":\"2026-10-15T16:38:39+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/\"},\"wordCount\":916,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg\",\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/\",\"name\":\"Tool Steel Heat Treatment Temperature Ranges | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg\",\"datePublished\":\"2026-09-30T22:06:40+00:00\",\"dateModified\":\"2026-10-15T16:38:39+00:00\",\"description\":\"The hardening, annealing, carburizing, nitriding and stress relieving ranges for tool steel, with the heat sources above them and the subzero range below, from a tool and die handbook.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-heat-treatment-temperature-ranges\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Tool Steel Heat Treatment Temperature Ranges and Reference Points\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uc628\ub3c4 \ubc94\uc704 | Aobo Steel","description":"\uacf5\uad6c \ubc0f \uae08\ud615 \ud578\ub4dc\ubd81\uc5d0\uc11c \uacf5\uad6c\uac15\uc758 \ub2f4\uae08\uc9c8, \uc5b4\ub2d0\ub9c1, \uce68\ud0c4, \uc9c8\ud654, \uc751\ub825\uc81c\uac70 \uc628\ub3c4 \ubc94\uc704\uc640 \uadf8 \uc0c1\uc704 \uc5f4\uc6d0 \ubc0f \ud558\uc704 \uc11c\ube0c\uc81c\ub85c \ubc94\uc704\ub97c \uc81c\uc2dc\ud569\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-temperature-ranges\/","og_locale":"ko_KR","og_type":"article","og_title":"Tool Steel Heat Treatment Temperature Ranges and Reference Points","og_description":"The hardening, annealing, carburizing, nitriding and stress relieving ranges for tool steel, with the heat sources above them and the subzero range below, from a tool and die handbook.","og_url":"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-temperature-ranges\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:38:39+00:00","og_image":[{"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"5\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Tool Steel Heat Treatment Temperature Ranges and Reference Points","datePublished":"2026-09-30T22:06:40+00:00","dateModified":"2026-10-15T16:38:39+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/"},"wordCount":916,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg","inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/","url":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/","name":"\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uc628\ub3c4 \ubc94\uc704 | Aobo Steel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg","datePublished":"2026-09-30T22:06:40+00:00","dateModified":"2026-10-15T16:38:39+00:00","description":"\uacf5\uad6c \ubc0f \uae08\ud615 \ud578\ub4dc\ubd81\uc5d0\uc11c \uacf5\uad6c\uac15\uc758 \ub2f4\uae08\uc9c8, \uc5b4\ub2d0\ub9c1, \uce68\ud0c4, \uc9c8\ud654, \uc751\ub825\uc81c\uac70 \uc628\ub3c4 \ubc94\uc704\uc640 \uadf8 \uc0c1\uc704 \uc5f4\uc6d0 \ubc0f \ud558\uc704 \uc11c\ube0c\uc81c\ub85c \ubc94\uc704\ub97c \uc81c\uc2dc\ud569\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/"]}]},{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Heat-Treatment-Ranges-totten-fig-11-9-temperature-ranges-carbon-and-tool-steels.jpg"},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-heat-treatment-temperature-ranges\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Tool Steel Heat Treatment Temperature Ranges and Reference Points"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tool Steel Heat Treatment Temperature Ranges and Reference Points The temperature ranges tool steel is hardened, annealed, carburized, nitrided and stress relieved at, with the heat sources above them and the subzero range below, from a tool and die shop handbook. A reference summary of published practice and not an Aobo Steel specification. How to&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tool Steel Heat Treatment Temperature Ranges and Reference Points The temperature ranges tool steel is hardened, annealed, carburized, nitrided and stress relieved at, with the heat sources above them and the subzero range below, from a tool and die shop handbook. A reference summary of published practice and not an Aobo Steel specification. How to&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20425","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20425"}],"version-history":[{"count":8,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20425\/revisions"}],"predecessor-version":[{"id":22538,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20425\/revisions\/22538"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20425"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}