{"id":20284,"date":"2026-09-30T02:09:31","date_gmt":"2026-09-29T18:09:31","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20284"},"modified":"2026-11-01T22:38:12","modified_gmt":"2026-11-01T14:38:12","slug":"hot-work-tool-steel-physical-properties","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/hot-work-tool-steel-physical-properties\/","title":{"rendered":"\uc5f4\uac04 \uacf5\uad6c\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\uc5f4\uac04 \uacf5\uad6c\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">4\uc885\uc758 \ud06c\ub86c \uc5f4\uac04 \uacf5\uad6c\uac15\uc744 \uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc\uc640 \uc5f4\ucc98\ub9ac \uc0c1\ud0dc\uc5d0\uc11c \uce21\uc815\ud55c \ube44\uc5f4, \uc5f4\uc804\ub3c4\uc728, \ubc00\ub3c4, \uc804\uae30 \uc800\ud56d\ub960 \ubc0f \ud0c4\uc131 \uacc4\uc218. \uacf5\uac1c\ub41c \uc2e4\ubb34 \uc790\ub8cc\uc758 \ucc38\uace0 \uc694\uc57d\uc774\uba70 Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2d8.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc774 \uc218\uce58\ub4e4\uc758 \uc6a9\ub3c4<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ub2e4\uc774 \ube14\ub85d\uc740 \uc218\uce58\ub85c \uc124\uacc4\ub418\uace0 \uac00\uc5f4 \ubc0f \ub0c9\uac01\ub429\ub2c8\ub2e4. \ube44\uc5f4\uacfc \ubc00\ub3c4\ub294 \ube14\ub85d\uc744 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4\uae4c\uc9c0 \uc62c\ub9ac\ub294 \ub370 \ud544\uc694\ud55c \uc5d0\ub108\uc9c0\ub7c9\uacfc \ub178\uac00 \uacf5\uae09\ud574\uc57c \ud558\ub294 \uc5f4\ub7c9\uc744 \uacb0\uc815\ud569\ub2c8\ub2e4. \uc5f4\uc804\ub3c4\uc728\uc740 \ub2f4\uae08\uc9c8 \uc911 \ud45c\uba74\uc5d0\uc11c \uc5f4\uc774 \ube60\uc838\ub098\uac00\ub294 \uc18d\ub3c4\uc640 \ub2e8\uba74 \uc804\uccb4\uc5d0 \uac78\uce5c \uc628\ub3c4\ucc28\uac00 \uc5bc\ub9c8\ub098 \uae09\uaca9\ud574\uc9c0\ub294\uc9c0\ub97c \uacb0\uc815\ud569\ub2c8\ub2e4. \ud0c4\uc131 \uacc4\uc218\ub294 \ud074\ub7a8\ud551 \ubc0f \uc8fc\uc870 \ud558\uc911 \ud558\uc5d0\uc11c \ube14\ub85d\uc774 \uc5bc\ub9c8\ub098 \ubcc0\ud615\ub418\ub294\uc9c0\ub97c \uacb0\uc815\ud558\uba70, \uc804\uae30 \uc800\ud56d\ub960\uc740 \ub2e4\uc774\ub97c \ubc29\uc804 \uac00\uacf5\ud558\uac70\ub098 \uc804\uae30\uc801\uc73c\ub85c \uc704\uce58\ub97c \uc7a1\uc544\uc57c \ud560 \ub54c \uc911\uc694\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">All four grades in this set are chromium hot work steels. <a href=\"https:\/\/aobosteel.com\/ko\/1-2343-tool-steel\/\">1.2343<\/a> and 1.2344 are the compositions known in the AISI system as H11 and H13, and 1.2365 and 1.2367 are the members of the same family carrying more chromium and molybdenum. Everything below was measured on these four grades only, so a grade outside the set has to be judged from its own datasheet.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ube44\uc5f4 \uc6a9\ub7c9<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">1.2344\uc640 1.2365\uc758 \uacbd\uc6b0 \uac12\uc774 \uc804\uccb4 \ubc94\uc704\uc5d0\uc11c \uc628\ub3c4\uc5d0 \ub530\ub77c \uc0c1\uc2b9\ud569\ub2c8\ub2e4. 1.2343\uacfc 1.2367\uc5d0\uc11c\ub294 \uc57d 500~600 \u00b0C\uae4c\uc9c0 \uc0c1\uc2b9\ud55c \ud6c4 \uc57d\uac04 \ub2e4\uc2dc \ub0ae\uc544\uc9c0\ub294\ub370, \uc774\ub294 \ucd9c\ucc98\uc5d0 \uc778\uc1c4\ub41c \ud615\ud0dc\uc774\uba70 \uc778\uc1c4\ub41c \uadf8\ub300\ub85c \uc7ac\ud604\ud55c \uac83\uc785\ub2c8\ub2e4. \ub124 \uac15\uc885 \uac04\uc758 \ud3b8\ucc28\ub294 100 \u00b0C\uc5d0\uc11c \uc57d 150 J\/kg\u00b7K\uc774\uace0 1000 \u00b0C\uc5d0\uc11c \uc57d 75 J\/kg\u00b7K\ub85c \uc881\ud600\uc9c0\ubbc0\ub85c, \uc0c1\uc628\uc5d0\uc11c \uc218\ud589\ud55c \ub178 \uacc4\uc0b0\uc740 \uc774 \uac15\uc885\ub4e4 \uac04\uc758 \ucc28\uc774\ub97c \uacfc\ub300\ud3c9\uac00\ud558\uac8c \ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc\uc758 \ube44\uc5f4, J\/kg\u00b7K<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uac15\uc885<\/th><th class=\"has-text-align-left\" data-align=\"left\">100 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">150 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">200 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">250 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">300 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">350 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">400 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">500 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">600 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">700 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">800 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">900 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">1000 \u00b0C<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2343<\/td><td class=\"has-text-align-left\" data-align=\"left\">523<\/td><td class=\"has-text-align-left\" data-align=\"left\">525<\/td><td class=\"has-text-align-left\" data-align=\"left\">530<\/td><td class=\"has-text-align-left\" data-align=\"left\">532<\/td><td class=\"has-text-align-left\" data-align=\"left\">535<\/td><td class=\"has-text-align-left\" data-align=\"left\">540<\/td><td class=\"has-text-align-left\" data-align=\"left\">540<\/td><td class=\"has-text-align-left\" data-align=\"left\">544<\/td><td class=\"has-text-align-left\" data-align=\"left\">544<\/td><td class=\"has-text-align-left\" data-align=\"left\">544<\/td><td class=\"has-text-align-left\" data-align=\"left\">544<\/td><td class=\"has-text-align-left\" data-align=\"left\">536<\/td><td class=\"has-text-align-left\" data-align=\"left\">536<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2344<\/td><td class=\"has-text-align-left\" data-align=\"left\">523<\/td><td class=\"has-text-align-left\" data-align=\"left\">545<\/td><td class=\"has-text-align-left\" data-align=\"left\">555<\/td><td class=\"has-text-align-left\" data-align=\"left\">580<\/td><td class=\"has-text-align-left\" data-align=\"left\">595<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">607<\/td><td class=\"has-text-align-left\" data-align=\"left\">615<\/td><td class=\"has-text-align-left\" data-align=\"left\">615<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">624<\/td><td class=\"has-text-align-left\" data-align=\"left\">628<\/td><td class=\"has-text-align-left\" data-align=\"left\">628<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2365<\/td><td class=\"has-text-align-left\" data-align=\"left\">481<\/td><td class=\"has-text-align-left\" data-align=\"left\">490<\/td><td class=\"has-text-align-left\" data-align=\"left\">505<\/td><td class=\"has-text-align-left\" data-align=\"left\">520<\/td><td class=\"has-text-align-left\" data-align=\"left\">530<\/td><td class=\"has-text-align-left\" data-align=\"left\">535<\/td><td class=\"has-text-align-left\" data-align=\"left\">545<\/td><td class=\"has-text-align-left\" data-align=\"left\">553<\/td><td class=\"has-text-align-left\" data-align=\"left\">553<\/td><td class=\"has-text-align-left\" data-align=\"left\">553<\/td><td class=\"has-text-align-left\" data-align=\"left\">553<\/td><td class=\"has-text-align-left\" data-align=\"left\">553<\/td><td class=\"has-text-align-left\" data-align=\"left\">553<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2367<\/td><td class=\"has-text-align-left\" data-align=\"left\">536<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">565<\/td><td class=\"has-text-align-left\" data-align=\"left\">575<\/td><td class=\"has-text-align-left\" data-align=\"left\">585<\/td><td class=\"has-text-align-left\" data-align=\"left\">595<\/td><td class=\"has-text-align-left\" data-align=\"left\">610<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">607<\/td><td class=\"has-text-align-left\" data-align=\"left\">599<\/td><td class=\"has-text-align-left\" data-align=\"left\">595<\/td><td class=\"has-text-align-left\" data-align=\"left\">582<\/td><td class=\"has-text-align-left\" data-align=\"left\">584<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ud480\ub9bc \uc0c1\ud0dc\uc758 \ube44\uc5f4, \ubcf4\uace0\uc11c\uc758 \ubb3c\uc131 \uc138\ud2b8-26 \ud56d\ubaa9 1.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uac12\uc740 J\/kg\u00b7K\uc774\uba70 \ucd9c\ucc98\uc5d0 \uba85\uc2dc\ub41c \ub300\ub85c \uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc\uc5d0 \uc801\uc6a9\ub429\ub2c8\ub2e4. \ucc38\uace0 \ud45c\uc77c \ubfd0\uc774\uba70 Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc5f4\uc804\ub3c4\uc728<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc804\ub3c4\uc728\uc740 \uc870\uc9c1\uc744 \ub530\ub974\ubbc0\ub85c \ub450 \uac00\uc9c0 \uc0c1\ud0dc\ub85c \uc81c\uc2dc\ub429\ub2c8\ub2e4. \ub124 \uac15\uc885 \ubaa8\ub450\uc5d0\uc11c \uc5f4\ucc98\ub9ac\ub41c \ubd09\uc7ac\ub294 \uc5b4\ub2d0\ub9c1\ub41c \ubd09\uc7ac\ubcf4\ub2e4 \uc804\ub3c4\uc728\uc774 \ub0ae\uc73c\uba70, \uc5ec\uae30\uc11c \uce21\uc815\ub41c \ubc94\uc704 \uc804\uccb4\uc5d0 \uac78\uccd0 \uc57d 1~3 W\/m\u00b7K \uc815\ub3c4 \ub0ae\uc2b5\ub2c8\ub2e4. \uc774\ub294 \ub2e4\uc774 \ud45c\uba74\uc774 \ub2f4\uae08\uc9c8 \ub9e4\uccb4\ub85c \uc5f4\uc744 \uc5bc\ub9c8\ub098 \ube68\ub9ac \uc804\ub2ec\ud560 \uc218 \uc788\ub294\uc9c0, \uadf8\ub9ac\uace0 \ud45c\uba74 \uc628\ub3c4 \uc911 \uc5bc\ub9c8\ub098 \ub9ce\uc740 \ubd80\ubd84\uc774 \uc804\uba74\uc758 \ub9e4\uccb4\uac00 \uc544\ub2cc \ud6c4\uba74\uc758 \uac15\uc7ac\uc5d0 \uc758\ud574 \uc804\ub2ec\ub418\ub294\uc9c0\ub97c \uacb0\uc815\ud558\ub294 \ud2b9\uc131\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\uc5b4\ub2d0\ub9c1 \ubc0f \uc5f4\ucc98\ub9ac \uc0c1\ud0dc\uc758 \uc5f4\uc804\ub3c4\uc728, W\/m\u00b7K<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uac15\uc885<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\ud0dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">100 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">200 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">300 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">400 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">500 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">600 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">700 \u00b0C<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2343<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.85<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.73<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.98<\/td><td class=\"has-text-align-left\" data-align=\"left\">31.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">31.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.32<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.41<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2343<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ucc98\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.84<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.47<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.26<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.31<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.35<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2344<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.09<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.22<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.14<\/td><td class=\"has-text-align-left\" data-align=\"left\">31.74<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">36.51<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2344<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ucc98\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.47<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.86<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.89<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.99<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.25<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2365<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.87<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.96<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.49<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.24<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.20<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2365<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ucc98\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">31.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.91<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">31.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.14<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.73<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.31<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2367<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.56<\/td><td class=\"has-text-align-left\" data-align=\"left\">31.82<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.66<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.49<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.17<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2367<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ucc98\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.94<\/td><td class=\"has-text-align-left\" data-align=\"left\">31.19<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.24<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.91<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.17<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \uc5f4\uc804\ub3c4\uc728, \ubcf4\uace0\uc11c\uc758 \ubb3c\uc131 \uc138\ud2b8-27 \ud56d\ubaa9 4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uac12\uc740 W\/m\u00b7K\uc785\ub2c8\ub2e4. \uc5f4\ucc98\ub9ac\ub780 43~44 HRC\ub85c \ub2f4\uae08\uc9c8 \ubc0f \ud15c\ud37c\ub9c1\ud55c \uac83\uc744 \uc758\ubbf8\ud558\uba70, \uc774\ub294 \ucd9c\ucc98\uac00 \uc790\uccb4 \uc218\uce58\ub97c \uc778\uc6a9\ud55c \uc0c1\ud0dc\uc785\ub2c8\ub2e4. \ucc38\uace0 \ud45c\uc77c \ubfd0\uc774\uba70 Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ubc00\ub3c4 \ubc0f \uc804\uae30 \uc800\ud56d\ub960<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ubc00\ub3c4\ub294 \uc138 \uac00\uc9c0 \uc0c1\ud0dc\ub85c \uc81c\uc2dc\ub429\ub2c8\ub2e4. \uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1\uc740 \uc5b4\ub2d0\ub9c1 \uac12\uc5d0 \ube44\ud574 \ubc00\ub3c4\ub97c \uc57d\uac04 \ub0ae\ucd94\ub294\ub370, \uc57d 7.73~7.85\ub97c \uae30\uc900\uc73c\ub85c 0.010~0.024 \uc815\ub3c4\uc774\uba70, \uc774\ub807\uac8c \uc791\uc740 \ubcc0\ud654\ub294 \uacf5\uce6d \ubc00\ub3c4\ub85c \uc218\ud589\ud55c \uc911\ub7c9 \uacc4\uc0b0\uc758 \uacf5\ucc28 \ubc94\uc704 \ub0b4\uc5d0 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\uc138 \uac00\uc9c0 \uc0c1\ud0dc\uc758 \ubc00\ub3c4, kg\/m\u00b3 \u00f7 1000<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uac15\uc885<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ud654<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ucc98\ub9ac<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2343<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.751<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.740<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.741<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2344<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.735<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.730<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.718<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2365<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.847<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.843<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.823<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2367<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.817<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.805<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.799<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ubc00\ub3c4, \ubcf4\uace0\uc11c\uc758 \ubb3c\uc131 \uc138\ud2b8-26 \ud56d\ubaa9 2.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uac12\uc740 kg\/m\u00b3\uc744 1000\uc73c\ub85c \ub098\ub208 \uac12\uc774\ubbc0\ub85c, 7.751\uc740 7751 kg\/m\u00b3\uc73c\ub85c \uc77d\uc2b5\ub2c8\ub2e4. \ucc38\uace0 \ud45c\uc77c \ubfd0\uc774\uba70 Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc800\ud56d\ub960\uc740 \uc5b4\ub2d0\ub9c1 \ubc0f \uc5f4\ucc98\ub9ac \uc0c1\ud0dc\uc5d0\uc11c 20 \u00b0C \uae30\uc900\uc73c\ub85c \uc81c\uc2dc\ub418\uba70, \ub124 \uac15\uc885 \ubaa8\ub450\uc5d0\uc11c \uacbd\ud654 \uc2dc \uc0c1\uc2b9\ud569\ub2c8\ub2e4. \uc138\ud2b8 \ub0b4 \ucd5c\uace0\uac12\uc740 \ucd5c\uc800\uac12\ubcf4\ub2e4 \uc57d 75\ud37c\uc13c\ud2b8 \ub192\uc73c\ubbc0\ub85c, \uc774\ub294 \uac15\uc885\ub4e4\uc744 \uadf8\ub8f9\ud654\ud558\uae30\ubcf4\ub2e4 \uad6c\ubd84\ud558\ub294 \uc218\uce58\uc785\ub2c8\ub2e4. \uac12\uc740 \ub9c8\uc774\ud06c\ub85c\uc634 \ubbf8\ud130\ub85c \uc81c\uc2dc\ub418\uba70, \uc774\ub294 1\uc634 \ubbf8\ud130\uc758 \ubc31\ub9cc\ubd84\uc758 1\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">20 \u00b0C\uc5d0\uc11c\uc758 \ube44\uc804\uae30 \uc800\ud56d\ub960, \ub9c8\uc774\ud06c\ub85c\uc634 \ubbf8\ud130<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uac15\uc885<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ucc98\ub9ac<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2343<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.471<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.481<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2344<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.520<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.532<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2365<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.303<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.308<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2367<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.366<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.397<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ube44\uc804\uae30\uc800\ud56d, \ubcf4\uace0\uc11c\uc758 \ubb3c\uc131 \uc138\ud2b8-27 \ud56d\ubaa9 5.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uac12\uc740 \ub9c8\uc774\ud06c\ub85c\uc634 \ubbf8\ud130, \uc989 1\uc634 \ubbf8\ud130\uc758 \ubc31\ub9cc\ubd84\uc758 1\uc785\ub2c8\ub2e4. \ucd9c\ucc98\ub294 \ub3d9\uc77c\ud55c \uc138\ud2b8\ub97c 4.71, 4.81, 5.20, 5.32, 3.03, 3.08, 3.66, 3.97\ub85c \uc778\uc1c4\ud558\uba70, \uac01\uac01 10\uc758 \ub9c8\uc774\ub108\uc2a4 7\uc2b9 \uc634 \ubbf8\ud130\ub97c \uacf1\ud55c \uac12\uc774\uace0, \uc5ec\uae30\uc11c \uc5ec\ub35f \uac12\uc758 \uc21c\uc11c\ub294 \ubcc0\uacbd\ub418\uc9c0 \uc54a\uc558\uc2b5\ub2c8\ub2e4. \ucc38\uace0 \ud45c\uc77c \ubfd0\uc774\uba70 Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud0c4\uc131\uacc4\uc218<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uacc4\uc218\ub294 \uc138 \uac00\uc9c0 \uc0c1\ud0dc\uc5d0\uc11c \uc0c1\uc628 \uae30\uc900\uc73c\ub85c \uc81c\uc2dc\ub429\ub2c8\ub2e4. \uacbd\ud654\uac00 \uac00\ub2a5\ud560 \uc815\ub3c4\ub85c \ube60\ub974\uac8c \ube14\ub85d\uc744 \ub0c9\uac01\ud558\uba74 \uc0c1\uc628 \uacc4\uc218\uac00 \uc5b4\ub2d0\ub9c1 \uac12\ubcf4\ub2e4 \ub0ae\uc544\uc9c0\ub294\ub370, \uac15\uc885\uc5d0 \ub530\ub77c \uc57d 9~21 kN\/mm\u00b2 \uc815\ub3c4 \ub0ae\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">20 \u00b0C\uc5d0\uc11c\uc758 \ud0c4\uc131 \uacc4\uc218, \uc81c\uacf1\ubc00\ub9ac\ubbf8\ud130\ub2f9 N\uc744 1000\uc73c\ub85c \ub098\ub208 \uac12<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uac15\uc885<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ud654<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ucc98\ub9ac<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2343<\/td><td class=\"has-text-align-left\" data-align=\"left\">217.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">206.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">215.6<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2344<\/td><td class=\"has-text-align-left\" data-align=\"left\">216.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">207.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">216.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2365<\/td><td class=\"has-text-align-left\" data-align=\"left\">217.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">208.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">213.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2367<\/td><td class=\"has-text-align-left\" data-align=\"left\">227.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">205.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">215.7<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, 20 \u00b0C\uc5d0\uc11c\uc758 \ud0c4\uc131\uacc4\uc218, \ubcf4\uace0\uc11c\uc758 \ubb3c\uc131 \uc138\ud2b8-27 \ud56d\ubaa9 6.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uac12\uc740 \uc81c\uacf1\ubc00\ub9ac\ubbf8\ud130\ub2f9 N\uc744 1000\uc73c\ub85c \ub098\ub208 \uac12\uc774\ubbc0\ub85c, 217.3\uc740 217300 N\/\uc81c\uacf1\ubc00\ub9ac\ubbf8\ud130\ub85c \uc77d\uc2b5\ub2c8\ub2e4. \ucc38\uace0 \ud45c\uc77c \ubfd0\uc774\uba70, Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc628\ub3c4\uc5d0 \ub530\ub77c \ud0c4\uc131 \uacc4\uc218\ub294 \uafb8\uc900\ud788 \uac10\uc18c\ud558\uba70 \ub124 \uac00\uc9c0 \uac15\uc885\uc740 \uc11c\ub85c \uadfc\uc811\ud55c \uac12\uc744 \uc720\uc9c0\ud569\ub2c8\ub2e4. 700 \u00b0C\uc5d0\uc11c \uac12\uc774 \ud45c\uae30\ub41c \ub450 \uac15\uc885\uc758 \uacbd\uc6b0 20\uc5d0\uc11c 700 \u00b0C\ub85c \uac08 \ub54c \uac10\uc18c\ud3ed\uc740 52~55 kN\/\uc81c\uacf1\ubc00\ub9ac\ubbf8\ud130\ub85c, \uc57d 4\ubd84\uc758 1 \uac10\uc18c\uc785\ub2c8\ub2e4. \uc774\uac83\uc774 \ub3d9\uc77c \ud558\uc911\uc5d0\uc11c \uc5f4\uac04 \ub2e4\uc774 \ube14\ub85d\uc774 \ub0c9\uac04 \ub2e4\uc774 \ube14\ub85d\ubcf4\ub2e4 \ub354 \ub9ce\uc774 \ubcc0\ud615\ub418\ub294 \uc774\uc720\uc774\uba70, \uace0\uc628\uc5d0\uc11c \uc791\ub3d9\ud558\ub294 \ube14\ub85d\uc758 \ubcc0\ud615 \uacc4\uc0b0\uc5d0 \ub123\uc5b4\uc57c \ud560 \uc218\uce58\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\uc5f4\ucc98\ub9ac \uc0c1\ud0dc\uc5d0\uc11c \uc2dc\ud5d8 \uc628\ub3c4\uc5d0 \ub530\ub978 \ud0c4\uc131 \uacc4\uc218<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uac15\uc885<\/th><th class=\"has-text-align-left\" data-align=\"left\">20 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">100 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">200 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">300 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">400 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">500 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">600 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">700 \u00b0C<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2343<\/td><td class=\"has-text-align-left\" data-align=\"left\">215.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">211.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">205.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">198.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">192.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">184.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">173.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">n\/a<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2344<\/td><td class=\"has-text-align-left\" data-align=\"left\">216.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">211.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">205.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">199.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">193.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">184.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">173.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">161.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2365<\/td><td class=\"has-text-align-left\" data-align=\"left\">213.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">209.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">202.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">196.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">191.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">183.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">173.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">160.9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.2367<\/td><td class=\"has-text-align-left\" data-align=\"left\">215.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">212.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">205.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">199.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">193.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">185.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">174.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">n\/a<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \uc5f4\ucc98\ub9ac \uc0c1\ud0dc\uc5d0\uc11c \uc2dc\ud5d8 \uc628\ub3c4\uc5d0 \ub530\ub978 \ud0c4\uc131\uacc4\uc218, \ubcf4\uace0\uc11c\uc758 \ubb3c\uc131 \uc138\ud2b8-27 \ud56d\ubaa9 7.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uac12\uc740 \uc81c\uacf1\ubc00\ub9ac\ubbf8\ud130\ub2f9 N\uc744 1000\uc73c\ub85c \ub098\ub208 \uac12\uc785\ub2c8\ub2e4. \ucd9c\ucc98\uc5d0 \ub450 \uc140\uc758 \uac12\uc774 \uc5c6\uc5b4 \uc5ec\uae30\uc11c\ub294 n\/a\ub85c \ud45c\uc2dc\ud588\uc2b5\ub2c8\ub2e4. \ucc38\uace0 \ud45c\uc77c \ubfd0\uc774\uba70, Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud45c \uc77d\ub294 \ubc29\ubc95<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc804\ub3c4\ub3c4, \ube44\uc800\ud56d \ubc0f \ud0c4\uc131 \uacc4\uc218 \ud45c\uc5d0\uc11c \uc5f4\ucc98\ub9ac \uc0c1\ud0dc\ub780 43~44 HRC\ub85c \ub2f4\uae08\uc9c8 \ubc0f \ub728\uc784\ud55c \uac83\uc744 \uc758\ubbf8\ud558\uba70, \uc774\ub294 \ucd9c\ucc98\uac00 \uc790\uccb4 \uc218\uce58\uc5d0 \ub300\ud574 \uba85\uc2dc\ud55c \ub0b4\uc6a9\uc785\ub2c8\ub2e4. \ub354 \ub192\uc740 \uacbd\ub3c4\ub85c \uc0ac\uc6a9\ub418\ub294 \ub2e4\uc774\ub294 \uc774 \uc218\uce58\ub97c \uc815\ud655\ud788 \ub530\ub974\uc9c0 \uc54a\uc73c\uba70, \uc9c8\ud654 \ucc98\ub9ac\ub41c \ub2e4\uc774\ub3c4 \ub9c8\ucc2c\uac00\uc9c0\uc785\ub2c8\ub2e4. \uc9c8\ud654\ub294 \uc5f0\ud55c \uc2ec\ubd80 \uc704\uc5d0 \uacbd\ud654\uce35\uc744 \ud615\uc131\ud558\uace0 \uadf8 \uacbd\ud654\uce35\uc740 \uace0\uc720\uc758 \ubb3c\uc131\uc744 \uac16\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud0c4\uc131 \uacc4\uc218 \ud45c\uc758 \ub450 \uc140\uc5d0\ub294 \uac12\uc774 \uc5c6\uc73c\uba70, 700 \u00b0C\uc5d0\uc11c 1.2343 \ubc0f 1.2367\uc5d0 \ud574\ub2f9\ud569\ub2c8\ub2e4. \ucd9c\ucc98\uc5d0 \uc544\ubb34 \uac12\ub3c4 \uc778\uc1c4\ub418\uc5b4 \uc788\uc9c0 \uc54a\uc544 n\/a\ub85c \ud45c\uc2dc\ud588\uc2b5\ub2c8\ub2e4. 1.2367\uc758 \uc5f4\ucc98\ub9ac \uc804\ub3c4\ub3c4 \uc5ed\uc2dc 600 \ubc0f 700 \u00b0C\uc5d0\uc11c \uc790\uccb4 \ud480\ub9bc \uac12\uc5d0 \uc218\ub834\ud558\uba70, \uc774\ub294 \ucd9c\ucc98\uac00 \uadf8 \uc30d\uc744 \uc778\uc1c4\ud55c \ubc29\uc2dd\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uc5f4\uac04 \uacf5\uad6c\uac15 \ubb3c\uc131, \uc778\uc1c4 \uac00\ub2a5\ud55c PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uc774 \ud398\uc774\uc9c0\uc758 \uc5ec\uc12f \uac1c \ud45c \ubaa8\ub450, 1.2343, 1.2344, 1.2365 \ubc0f 1.2367\uc758 \ube44\uc5f4, \uc5f4\uc804\ub3c4\ub3c4, \ubc00\ub3c4, \uc804\uae30 \ube44\uc800\ud56d \ubc0f \ud0c4\uc131 \uacc4\uc218\ub97c \uc800\ud76c \uc5f0\ub77d\ucc98 \uc815\ubcf4\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Hot-Work-Tool-Steel-Physical-Properties.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 449 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ub370\uc774\ud130<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \uc5f4 \uc911 \ub450 \uac1c\uc758 \uae30\ubc18\uc774 \ub418\ub294 \uac15\uc885\uc740 \ub2e4\uc74c\uc5d0 \uc815\ub9ac\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel\/\">H13 \uacf5\uad6c\uac15 \ud398\uc774\uc9c0<\/a> \ubc0f <a href=\"https:\/\/aobosteel.com\/ko\/h11-tool-steel\/\">H11 \uacf5\uad6c\uac15 \ud398\uc774\uc9c0<\/a>, \uadf8\ub9ac\uace0 \uc5f4\ucc98\ub9ac \uc0c1\ud0dc\ub97c \ub9cc\ub4dc\ub294 \uc0ac\uc774\ud074\uc740 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/h13-steel-heat-treatment\/\">H13 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc<\/a>. \ud2b9\uc815 \ub2e4\uc774\uc5d0 \ub300\ud55c 1.2344\uc640 1.2367\uc758 \ucc28\uc774\ub294 \ub2e4\uc74c \ud398\uc774\uc9c0\uc5d0\uc11c \uc790\uc138\ud788 \ub2e4\ub8f9\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/h13-vs-1-2367-tool-steel\/\">H13 \ub300 1.2367 \ud398\uc774\uc9c0<\/a>. \ub354 \ub9ce\uc740 \uacf5\uad6c\uac15 \uac15\uc885\uc758 \ud3c9\uade0 \uc5f4\ud33d\ucc3d \ubc0f \ubc00\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-density-thermal-expansion\/\">\ubc00\ub3c4 \ubc0f \uc5f4\ud33d\ucc3d \ucc28\ud2b8<\/a>, \uadf8\ub9ac\uace0 \ub2e4\ub978 \uc77c\uacf1 \uac15\uc885\uc758 \uc804\ub3c4\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-thermal-conductivity\/\">\uc5f4\uc804\ub3c4\ub3c4 \ucc28\ud2b8<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: Improved Life of Die Casting Dies of H13 Steel by Attaining Improved Mechanical Properties and Distortion Control During Heat Treatment (J. F. Wallace and D. Schwam, US Department of Energy final report DOE\/ID\/13320-3, October 1998).<\/p>","protected":false},"excerpt":{"rendered":"<p>Hot Work Tool Steel Physical Properties Specific heat capacity, thermal conductivity, density, electrical resistivity and modulus of elasticity measured in four chromium hot work tool steels, in the annealed and the heat treated condition. A reference summary of published practice and not an Aobo Steel specification. What these figures are used for A die block [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20284","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Hot Work Tool Steel Physical Properties 1.2343 1.2367<\/title>\n<meta name=\"description\" content=\"Specific heat, thermal conductivity, density, electrical resistivity and elastic modulus measured in hot work tool steels 1.2343, 1.2344, 1.2365 and 1.2367.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/hot-work-tool-steel-physical-properties\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Hot Work Tool Steel Physical Properties\" \/>\n<meta property=\"og:description\" content=\"Specific heat, thermal conductivity, density, electrical resistivity and elastic modulus measured in hot work tool steels 1.2343, 1.2344, 1.2365 and 1.2367.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/hot-work-tool-steel-physical-properties\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-11-01T14:38:12+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"7\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hot-work-tool-steel-physical-properties\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hot-work-tool-steel-physical-properties\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Hot Work Tool Steel Physical Properties\",\"datePublished\":\"2026-09-29T18:09:31+00:00\",\"dateModified\":\"2026-11-01T14:38:12+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hot-work-tool-steel-physical-properties\\\/\"},\"wordCount\":1319,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hot-work-tool-steel-physical-properties\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/hot-work-tool-steel-physical-properties\\\/\",\"name\":\"Hot Work Tool Steel Physical Properties 1.2343 1.2367\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-29T18:09:31+00:00\",\"dateModified\":\"2026-11-01T14:38:12+00:00\",\"description\":\"Specific heat, thermal conductivity, density, electrical resistivity and elastic modulus measured in hot work tool steels 1.2343, 1.2344, 1.2365 and 1.2367.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hot-work-tool-steel-physical-properties\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/hot-work-tool-steel-physical-properties\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hot-work-tool-steel-physical-properties\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Hot Work Tool Steel Physical Properties\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uc5f4\uac04 \uacf5\uad6c\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131 1.2343 1.2367","description":"\uc5f4\uac04 \uacf5\uad6c\uac15 1.2343, 1.2344, 1.2365, 1.2367\uc5d0\uc11c \uce21\uc815\ud55c \ube44\uc5f4, \uc5f4\uc804\ub3c4\uc728, \ubc00\ub3c4, \uc804\uae30 \uc800\ud56d\ub960 \ubc0f \ud0c4\uc131\uacc4\uc218\ub97c \uc81c\uc2dc\ud569\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/hot-work-tool-steel-physical-properties\/","og_locale":"ko_KR","og_type":"article","og_title":"Hot Work Tool Steel Physical Properties","og_description":"Specific heat, thermal conductivity, density, electrical resistivity and elastic modulus measured in hot work tool steels 1.2343, 1.2344, 1.2365 and 1.2367.","og_url":"https:\/\/aobosteel.com\/ko\/hot-work-tool-steel-physical-properties\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-11-01T14:38:12+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"7\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/hot-work-tool-steel-physical-properties\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/hot-work-tool-steel-physical-properties\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Hot Work Tool Steel Physical Properties","datePublished":"2026-09-29T18:09:31+00:00","dateModified":"2026-11-01T14:38:12+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/hot-work-tool-steel-physical-properties\/"},"wordCount":1319,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/hot-work-tool-steel-physical-properties\/","url":"https:\/\/aobosteel.com\/hot-work-tool-steel-physical-properties\/","name":"\uc5f4\uac04 \uacf5\uad6c\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131 1.2343 1.2367","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-29T18:09:31+00:00","dateModified":"2026-11-01T14:38:12+00:00","description":"\uc5f4\uac04 \uacf5\uad6c\uac15 1.2343, 1.2344, 1.2365, 1.2367\uc5d0\uc11c \uce21\uc815\ud55c \ube44\uc5f4, \uc5f4\uc804\ub3c4\uc728, \ubc00\ub3c4, \uc804\uae30 \uc800\ud56d\ub960 \ubc0f \ud0c4\uc131\uacc4\uc218\ub97c \uc81c\uc2dc\ud569\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/hot-work-tool-steel-physical-properties\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/hot-work-tool-steel-physical-properties\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/hot-work-tool-steel-physical-properties\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Hot Work Tool Steel Physical Properties"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Hot Work Tool Steel Physical Properties Specific heat capacity, thermal conductivity, density, electrical resistivity and modulus of elasticity measured in four chromium hot work tool steels, in the annealed and the heat treated condition. A reference summary of published practice and not an Aobo Steel specification. What these figures are used for A die block&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Hot Work Tool Steel Physical Properties Specific heat capacity, thermal conductivity, density, electrical resistivity and modulus of elasticity measured in four chromium hot work tool steels, in the annealed and the heat treated condition. A reference summary of published practice and not an Aobo Steel specification. What these figures are used for A die block&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20284","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20284"}],"version-history":[{"count":6,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20284\/revisions"}],"predecessor-version":[{"id":24896,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20284\/revisions\/24896"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20284"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}