{"id":20276,"date":"2026-09-30T00:13:14","date_gmt":"2026-09-29T16:13:14","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20276"},"modified":"2026-10-16T00:20:16","modified_gmt":"2026-10-15T16:20:16","slug":"h13-steel-microstructure-after-quenching","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/h13-steel-microstructure-after-quenching\/","title":{"rendered":"H13 \uac15 \ub2f4\uae08\uc9c8 \ud6c4 \ubbf8\uc138\uc870\uc9c1"},"content":{"rendered":"<h1 class=\"wp-block-heading\">H13 \uac15 \ub2f4\uae08\uc9c8 \ud6c4 \ubbf8\uc138\uc870\uc9c1<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\uc9c4\uacf5, \uac00\uc2a4, \uc5fc\uc695, \uc624\uc77c \ubc0f \ud3f4\ub9ac\uba38\uc5d0\uc11c \ub2f4\uae08\uc9c8\ud55c H13 \ube14\ub85d\uc5d0\uc11c \uce21\uc815\ub41c \ud384\ub77c\uc774\ud2b8, \ubca0\uc774\ub098\uc774\ud2b8 \ubc0f \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\ub97c \uac01 \ub2f4\uae08\uc9c8 \uc870\uac74\uc758 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uacb0\uc815\ub9bd\uacc4\uc5d0\uc11c\uc758 MC \ud0c4\ud654\ubb3c \uc11d\ucd9c\uacfc \ud568\uaed8 \ub098\ud0c0\ub0b8\ub2e4. \ubc1c\ud45c\ub41c \uc2e4\ubb34\uc5d0 \ub300\ud55c \ucc38\uace0 \uc694\uc57d\uc774\uba70 Aobo Steel\uc758 \uaddc\uaca9\uc774 \uc544\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub2f4\uae08\uc9c8\uc774 \uacb0\uc815\ud558\ub294 \uac83<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">H13 \ub2e4\uc774\ub294 \uc57d 1010~1050 \u00b0C \uc601\uc5ed\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ub41c \ud6c4 \ubcc0\ud0dc \ubc94\uc704\ub97c \ud1b5\uacfc\ud558\uba70 \ub0c9\uac01\ub41c\ub2e4. \ub0c9\uac01 \uc911 \uac15\uc774 \uc5b4\ub5a4 \uc870\uc9c1\uc73c\ub85c \ubcc0\ud558\ub294\uc9c0\ub294 \ud574\ub2f9 \ubc94\uc704\ub97c \uc5bc\ub9c8\ub098 \ube60\ub974\uac8c \ud1b5\uacfc\ud558\ub294\uc9c0\uc5d0 \ub2ec\ub824 \uc788\uc73c\uba70, \ub450\uaebc\uc6b4 \ub2e8\uba74\uc740 \ud45c\uba74\uc5d0\uc11c \uc5f4\uc744 \ubc29\ucd9c\ud558\ub294 \uc18d\ub3c4\uac00 \uc2ec\ubd80\uc5d0\uc11c \uc5f4\uc744 \uacf5\uae09\ud558\ub294 \uc18d\ub3c4\ubcf4\ub2e4 \ube60\ub97c \uc218 \uc5c6\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \ub370\uc774\ud130\uc758 \uadfc\uac70\uac00 \ub41c \ubcf4\uace0\uc11c\ub294 \ub0c9\uac01 \uace1\uc120\uc744 \ub450 \uad6c\uac04\uc73c\ub85c \ub098\ub208\ub2e4. 1750~1550 \u00b0F \uc0ac\uc774\uc758 \uc18d\ub3c4\ub294 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uacb0\uc815\ub9bd\uacc4\uc5d0 \uc11d\ucd9c\ub418\ub294 MC \ud0c4\ud654\ubb3c\uc758 \uc591\uc744 \uacb0\uc815\ud55c\ub2e4. 1550~750 \u00b0F \uc0ac\uc774\uc758 \uc18d\ub3c4\ub294 \uae30\uc9c0 \uc870\uc9c1, \uc989 \ub2e4\uc774\uc5d0 \ucd5c\uc885\uc801\uc73c\ub85c \ub0a8\ub294 \ud384\ub77c\uc774\ud2b8, \ubca0\uc774\ub098\uc774\ud2b8 \ubc0f \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uc758 \uc591\uc744 \uacb0\uc815\ud55c\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub450 \uad6c\uac04 \ubaa8\ub450 \uc5f0\uad6c\uc5d0 \ud3ec\ud568\ub41c \ub450 \uadf9\ub2e8\uc801 \ube14\ub85d \ud06c\uae30\uc778 2\uc778\uce58 \ud050\ube0c\uc640 14\uc778\uce58 \ud050\ube0c\uc5d0 \ub300\ud574, \uc815\uc9c0 \uc9c4\uacf5\uc5d0\uc11c \ubb3d\uc740 \ud3f4\ub9ac\uba38 \uc6a9\uc561\uc5d0 \uc774\ub974\ub294 \uc5f4 \uac00\uc9c0 \ub2f4\uae08\uc9c8 \ub9e4\uccb4\uc5d0\uc11c \uce21\uc815\ub418\uc5c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub2f4\uae08\uc9c8 \ud6c4 \uae30\uc9c0 \ubbf8\uc138\uc870\uc9c1<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc218\uce58\ub294 \ube14\ub85d \ud45c\uba74\uacfc \uc911\uac04 \ubc18\uacbd\uc5d0\uc11c \uac01 \uc0c1\uc758 \ube44\uc728\uc774\ub2e4. B\ub294 \ubca0\uc774\ub098\uc774\ud2b8, M\uc740 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8, P\ub294 \ud384\ub77c\uc774\ud2b8\uc774\ub2e4. \uac00\uc2a4 \uacb0\uacfc\ub294 2 atm\uc5d0\uc11c \uac00\uc2a4 \uc18d\ub3c4 3,400 ft\/min\uc758 \uc9c8\uc18c \ubc0f \ud5ec\ub968\uc5d0 \ub300\ud55c \uac83\uc73c\ub85c, \ubcf4\uace0\uc11c\uac00 \uac00\uc2a4 \ub2f4\uae08\uc9c8\uc5d0 \uc0ac\uc6a9\ud55c \uc870\uac74\uc774\ub2e4. \uc5fc\uc695\uacfc \ub450 \ud3f4\ub9ac\uba38 \uc6a9\uc561\uc740 \uc774 \uc2dc\ub9ac\uc988\uc5d0\uc11c \uac00\uc7a5 \ube60\ub978 \ub9e4\uccb4\uc774\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4\ubcc4 \ud384\ub77c\uc774\ud2b8, \ubca0\uc774\ub098\uc774\ud2b8 \ubc0f \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4<\/th><th class=\"has-text-align-left\" data-align=\"left\">2\uc778\uce58 \ud050\ube0c \ud45c\uba74<\/th><th class=\"has-text-align-left\" data-align=\"left\">2\uc778\uce58 \ud050\ube0c \uc911\uac04 \ubc18\uacbd<\/th><th class=\"has-text-align-left\" data-align=\"left\">14\uc778\uce58 \ud050\ube0c \ud45c\uba74<\/th><th class=\"has-text-align-left\" data-align=\"left\">14\uc778\uce58 \ud050\ube0c \uc911\uac04 \ubc18\uacbd<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc9c4\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">28B 72M<\/td><td class=\"has-text-align-left\" data-align=\"left\">28B 72M<\/td><td class=\"has-text-align-left\" data-align=\"left\">13P 72B 15M<\/td><td class=\"has-text-align-left\" data-align=\"left\">14P 72B 14M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc9c8\uc18c<\/td><td class=\"has-text-align-left\" data-align=\"left\">16B 84M<\/td><td class=\"has-text-align-left\" data-align=\"left\">16B 84M<\/td><td class=\"has-text-align-left\" data-align=\"left\">42B 58M<\/td><td class=\"has-text-align-left\" data-align=\"left\">42B 58M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud5ec\ub968<\/td><td class=\"has-text-align-left\" data-align=\"left\">13B 87M<\/td><td class=\"has-text-align-left\" data-align=\"left\">13B 87M<\/td><td class=\"has-text-align-left\" data-align=\"left\">38B 62M<\/td><td class=\"has-text-align-left\" data-align=\"left\">38B 62M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc800\uc18d \uc624\uc77c<\/td><td class=\"has-text-align-left\" data-align=\"left\">7B 93M<\/td><td class=\"has-text-align-left\" data-align=\"left\">7B 93M<\/td><td class=\"has-text-align-left\" data-align=\"left\">26B 74M<\/td><td class=\"has-text-align-left\" data-align=\"left\">30B 70M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc720\ub3d9 \uc54c\ub8e8\ubbf8\ub098<\/td><td class=\"has-text-align-left\" data-align=\"left\">5B 95M<\/td><td class=\"has-text-align-left\" data-align=\"left\">5B 95M<\/td><td class=\"has-text-align-left\" data-align=\"left\">23B 77M<\/td><td class=\"has-text-align-left\" data-align=\"left\">29B 71M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uace0\uc18d \uc624\uc77c<\/td><td class=\"has-text-align-left\" data-align=\"left\">2B 98M<\/td><td class=\"has-text-align-left\" data-align=\"left\">2B 98M<\/td><td class=\"has-text-align-left\" data-align=\"left\">15B 85M<\/td><td class=\"has-text-align-left\" data-align=\"left\">27B 73M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">30% UCON A \uc6a9\uc561<\/td><td class=\"has-text-align-left\" data-align=\"left\">100M<\/td><td class=\"has-text-align-left\" data-align=\"left\">1B 99M<\/td><td class=\"has-text-align-left\" data-align=\"left\">8B 92M<\/td><td class=\"has-text-align-left\" data-align=\"left\">26B 74M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% UCON A \uc6a9\uc561<\/td><td class=\"has-text-align-left\" data-align=\"left\">100M<\/td><td class=\"has-text-align-left\" data-align=\"left\">100M<\/td><td class=\"has-text-align-left\" data-align=\"left\">100M<\/td><td class=\"has-text-align-left\" data-align=\"left\">25B 75M<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ub450 \uac00\uc9c0 \uadf9\ub2e8\uc801\uc778 H13 \uac15 \ube14\ub85d \ud06c\uae30\uc5d0 \ub300\ud55c \ub2f4\uae08\uc9c8 \ub9e4\uccb4\uc5d0 \ub530\ub77c \uc0dd\uc131\ub41c \uae30\uc9c0 \ubbf8\uc138\uc870\uc9c1, \ubcf4\uace0\uc11c\uc758 Table V-16.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>B\ub294 \ubca0\uc774\ub098\uc774\ud2b8, M\uc740 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8, P\ub294 \ud384\ub77c\uc774\ud2b8\uc774\uba70, \uac01 \uc140 \ub0b4\uc758 \uc218\uce58\ub294 \ubc31\ubd84\uc728\uc785\ub2c8\ub2e4. \ubcf4\uace0\uc11c\uc5d0 \ub530\ub974\uba74 2\uc778\uce58 \ube14\ub85d\uc758 \ud45c\uba74\uacfc \uc911\uac04 \ubc18\uacbd\uc740 \ubcf8\uc9c8\uc801\uc73c\ub85c \ub3d9\uc77c\ud569\ub2c8\ub2e4. \uac00\uc2a4 \uc218\uce58\ub294 2 atm\uc5d0\uc11c \uc9c8\uc18c\uc640 \ud5ec\ub968, \uac00\uc2a4 \uc18d\ub3c4 3,400 ft\/min\uc5d0 \ub300\ud55c \uac83\uc785\ub2c8\ub2e4. \ucc38\uace0\uc6a9 \ud45c\uc77c \ubfd0\uc774\uba70, Aobo Steel\uc758 \uad8c\uc7a5 \uc0ac\ud56d\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uacb0\uc815\ub9bd\uacc4\uc5d0\uc11c\uc758 \ud0c4\ud654\ubb3c \uc11d\ucd9c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">MC \ud0c4\ud654\ubb3c\uc740 \ube14\ub85d\uc774 1750~1550 \u00b0F \uc0ac\uc774\uc5d0 \uc788\ub294 \ub3d9\uc548 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uacb0\uc815\ub9bd\uacc4\uc5d0\uc11c \ud615\uc131\ub418\uba70, \ub290\ub9b0 \ub2f4\uae08\uc9c8\uc740 \uc774 \uc628\ub3c4 \ubc94\uc704 \ub0b4\uc5d0 \ub354 \uc624\ub798 \uba38\ubb3c\uac8c \ud569\ub2c8\ub2e4. \ubcf4\uace0\uc11c\ub294 \uadf8 \uc591\uc744 0~100 \ucc99\ub3c4\uc758 \uc218\uce58\ub85c \uc81c\uc2dc\ud558\uba70, \uc22b\uc790\uac00 \ub192\uc744\uc218\ub85d \uacbd\uacc4\uc5d0\uc11c \uc11d\ucd9c\uc774 \ub354 \ub9ce\uc74c\uc744 \uc758\ubbf8\ud569\ub2c8\ub2e4. \uacb0\uc815\ub9bd\uacc4 \ud0c4\ud654\ubb3c\uc740 \ub290\ub9b0 \ub2f4\uae08\uc9c8 \ud6c4\uc5d0 \ub098\ud0c0\ub098\ub294 \uc5f0\uc131 \ubc0f \ucda9\uaca9 \uc778\uc131 \uc800\ud558\uc758 \uc6d0\uc778\uc774\uba70, \ub530\ub77c\uc11c \uc774 \ud45c\ub294 \uc704\uc758 \ud45c\uc640 \ubc18\ub300 \ubc29\ud5a5\uc73c\ub85c \uc77d\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4\uc5d0 \ub530\ub978 MC \uacb0\uc815\ub9bd\uacc4 \uc11d\ucd9c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4<\/th><th class=\"has-text-align-left\" data-align=\"left\">2\uc778\uce58 \ud050\ube0c \ud45c\uba74<\/th><th class=\"has-text-align-left\" data-align=\"left\">2\uc778\uce58 \ud050\ube0c \uc911\uac04 \ubc18\uacbd<\/th><th class=\"has-text-align-left\" data-align=\"left\">14\uc778\uce58 \ud050\ube0c \ud45c\uba74<\/th><th class=\"has-text-align-left\" data-align=\"left\">14\uc778\uce58 \ud050\ube0c \uc911\uac04 \ubc18\uacbd<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc9c4\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">91<\/td><td class=\"has-text-align-left\" data-align=\"left\">91<\/td><td class=\"has-text-align-left\" data-align=\"left\">98<\/td><td class=\"has-text-align-left\" data-align=\"left\">98<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc9c8\uc18c<\/td><td class=\"has-text-align-left\" data-align=\"left\">74<\/td><td class=\"has-text-align-left\" data-align=\"left\">74<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><td class=\"has-text-align-left\" data-align=\"left\">96<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud5ec\ub968<\/td><td class=\"has-text-align-left\" data-align=\"left\">68<\/td><td class=\"has-text-align-left\" data-align=\"left\">68<\/td><td class=\"has-text-align-left\" data-align=\"left\">92<\/td><td class=\"has-text-align-left\" data-align=\"left\">96<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc800\uc18d \uc624\uc77c<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">750 \u00b0F \uc5fc\uc695<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc720\ub3d9 \uc54c\ub8e8\ubbf8\ub098<\/td><td class=\"has-text-align-left\" data-align=\"left\">44<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">51<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">575 \u00b0F \uc5fc\uc695<\/td><td class=\"has-text-align-left\" data-align=\"left\">28<\/td><td class=\"has-text-align-left\" data-align=\"left\">41<\/td><td class=\"has-text-align-left\" data-align=\"left\">32<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uace0\uc18d \uc624\uc77c<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">93<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">30% UCON A \uc6a9\uc561<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">27<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">92<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% UCON A \uc6a9\uc561<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">92<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, \ub450 \uac00\uc9c0 \uadf9\ub2e8\uc801\uc778 H13 \uac15 \ube14\ub85d \ud06c\uae30\uc5d0 \ub300\ud55c \ub2f4\uae08\uc9c8 \ub9e4\uccb4\uc5d0 \ub530\ub978 MC \uc785\uacc4 \uc11d\ucd9c, \ubcf4\uace0\uc11c\uc758 Table IV-15.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uc218\uce58\ub294 \ubcf4\uace0\uc11c\uc5d0\uc11c \uc0ac\uc6a9\ud558\ub294 0~100 \ucc99\ub3c4\uc774\uba70, \uc22b\uc790\uac00 \ub192\uc744\uc218\ub85d \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uacb0\uc815\ub9bd\uacc4\uc5d0\uc11c MC \ud0c4\ud654\ubb3c \uc11d\ucd9c\uc774 \ub354 \ub9ce\uc74c\uc744 \uc758\ubbf8\ud569\ub2c8\ub2e4. \ub450 \uac1c\uc758 \uc5fc\uc695 \ud56d\ubaa9\uc740 \uc774 \ud45c\uc5d0\ub9cc \ub098\ud0c0\ub098\uba70, 575 \u00b0F \uc5fc\uc695\uc774 \ub458 \uc911 \ub354 \ube60\ub985\ub2c8\ub2e4. \ucc38\uace0\uc6a9 \ud45c\uc77c \ubfd0\uc774\uba70, Aobo Steel\uc758 \uad8c\uc7a5 \uc0ac\ud56d\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub450 \ud45c\ub97c \ud568\uaed8 \uc77d\uae30<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">2\uc778\uce58 \ud050\ube0c\uc5d0\uc11c\ub294 \ud45c\uba74\uacfc \uc911\uac04 \ubc18\uacbd\uc758 \ud310\ub3c5\uac12\uc774 \ub3d9\uc77c\ud55c\ub370, \uadf8\ub807\uac8c \uc791\uc740 \ub2e8\uba74\uc740 \uc790\uccb4\uc801\uc73c\ub85c \uc628\ub3c4 \ucc28\uc774\ub97c \ucda9\ubd84\ud788 \uc624\ub798 \uc720\uc9c0\ud560 \uc218 \uc5c6\uc5b4 \ubb38\uc81c\uac00 \ub418\uc9c0 \uc54a\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uc9c4\uacf5 \ub2f4\uae08\uc9c8\ub294 \ubca0\uc774\ub098\uc774\ud2b8\uac00 \uac00\uc7a5 \ub9ce\uc774 \ub0a8\uc544 28% \ub300 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8 72%\ub97c \ubcf4\uc774\uba70, \ub0c9\uac01 \uc18d\ub3c4\uac00 \ud55c \ub2e8\uacc4\uc529 \uc62c\ub77c\uac08 \ub54c\ub9c8\ub2e4 \uadf8 \uc591\uc740 \uac10\uc18c\ud558\uc5ec \uace0\uc18d \uc624\uc77c\uc5d0\uc11c\ub294 2%\uac00 \ub429\ub2c8\ub2e4. \ub450 \ud3f4\ub9ac\uba38 \uc6a9\uc561 \ubaa8\ub450 \ud574\ub2f9 \ube14\ub85d\uc744 \uc644\uc804 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\ub85c \ub9cc\ub4ed\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">14\uc778\uce58 \ud050\ube0c\uc5d0\uc11c\ub294 \ub3d9\uc77c\ud55c \ub9e4\uccb4\uac00 \ub9e4\uc6b0 \ub2e4\ub974\uac8c \uac70\ub3d9\ud569\ub2c8\ub2e4. \uc911\uac04 \ubc18\uacbd\uc740 \ub2f4\uae08\uc9c8 \ubc29\uc2dd\uc5d0 \uad00\uacc4\uc5c6\uc774 25%\uc5d0\uc11c 72% \uc0ac\uc774\uc758 \ubca0\uc774\ub098\uc774\ud2b8\uc5d0 \uc704\uce58\ud558\ub294\ub370, \uc5f4\uc774 \uac15\uc7ac \uc790\uccb4\ub97c \ud1b5\ud574 \ube60\uc838\ub098\uac00\uc57c \ud558\uace0 \ud45c\uba74\uc774 \ucf54\uc5b4\ub97c \uc81c\uc5b4\ud558\uc9c0 \ubabb\ud558\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \ud45c\uba74\uc5d0\uc11c\ub294 10% UCON A \uc6a9\uc561\ub9cc\uc774 \uc644\uc804 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uc5d0 \ub3c4\ub2ec\ud558\uba70, \uc9c4\uacf5 \ub2f4\uae08\uc9c8\ub294 \ucda9\ubd84\ud788 \ub290\ub824 \ub450 \uc704\uce58 \ubaa8\ub450\uc5d0\uc11c \uc870\uc9c1\uc5d0 \ud384\ub77c\uc774\ud2b8\ub97c \ub0a8\uae41\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">MC \uc11d\ucd9c\uc740 \ubc18\ub300 \ubc29\ud5a5\uc73c\ub85c \uc9c4\ud589\ub429\ub2c8\ub2e4. \uc9c4\uacf5 \ub2f4\uae08\uc9c8\ub294 \ucc99\ub3c4\uc5d0\uc11c 91\uc5d0\uc11c 98\uc744 \uae30\ub85d\ud558\uace0, \ub450 \ud3f4\ub9ac\uba38 \uc6a9\uc561\uc740 \ub450 \ube14\ub85d\uc758 \ud45c\uba74\uc5d0\uc11c 0\uc744 \uae30\ub85d\ud569\ub2c8\ub2e4. 14\uc778\uce58 \ud050\ube0c\uc758 \uc911\uac04 \ubc18\uacbd\uc5d0\uc11c\ub294 \ubaa8\ub4e0 \ub2f4\uae08\uc9c8\uac00 92\uc5d0\uc11c 98 \uc0ac\uc774\uc5d0 \uc704\uce58\ud558\ub294\ub370, \uc774\ub294 \ub9e4\ud2b8\ub9ad\uc2a4 \ud45c\ub97c \ubc18\ub300 \ubc29\ud5a5\uc5d0\uc11c \uc77d\uc740 \uac83\uacfc \uac19\uc740 \uba54\uc2dc\uc9c0\ub85c, \ub450\uaebc\uc6b4 H13 \ube14\ub85d\uc758 \uc911\uc559\ubd80\ub294 \uac15\uc7ac\uc5d0 \uc758\ud574 \uacb0\uc815\ub418\uace0 \uc8fc\ubcc0 \ub9e4\uccb4\uc5d0 \uc758\ud574\uc11c\ub294 \uac70\uc758 \uc601\ud5a5\uc744 \ubc1b\uc9c0 \uc54a\ub294\ub2e4\ub294 \uac83\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\ub2f4\uae08\uc9c8 \ud6c4 H13 \uac15 \ubbf8\uc138\uc870\uc9c1, \uc778\uc1c4 \uac00\ub2a5\ud55c PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uc774 \ud398\uc774\uc9c0\uc758 \ub450 \ud45c, \ub450 \uadf9\ub2e8\uc801\uc778 H13 \ube14\ub85d \ud06c\uae30\uc5d0 \ub300\ud55c \uae30\uc9c0 \ubbf8\uc138\uc870\uc9c1\uacfc MC \uacb0\uc815\ub9bd\uacc4 \uc11d\ucd9c\uc744 \ub2f9\uc0ac \uc5f0\ub77d\ucc98\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-H13-Steel-Microstructure-After-Quenching.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 391 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ub370\uc774\ud130<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \ub370\uc774\ud130\uac00 \uc18d\ud558\ub294 \uac15\uc885\uc740 \ub2e4\uc74c \ud398\uc774\uc9c0\uc5d0 \uc124\uba85\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel\/\">H13 \uacf5\uad6c\uac15 \ud398\uc774\uc9c0<\/a>, \uadf8\ub9ac\uace0 \uc774\ub7ec\ud55c \ubbf8\uc138\uc870\uc9c1 \ub4a4\uc5d0 \uc788\ub294 \ub0c9\uac01 \uc18d\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/h13-quenching-cooling-rates\/\">H13 \ub2f4\uae08\uc9c8 \ub0c9\uac01 \uc18d\ub3c4 \ud398\uc774\uc9c0<\/a>. \ub2f4\uae08\uc9c8 \uc8fc\ubcc0\uc758 \ub098\uba38\uc9c0 \uc0ac\uc774\ud074\uc740 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/h13-steel-heat-treatment\/\">H13 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc<\/a>, \ub3c4\ub2ec\ud574\uc57c \ud558\ub294 \uc0ac\uc6a9 \uacbd\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/h13-steel-hardness\/\">H13 \uacbd\ub3c4 \ucc28\ud2b8<\/a>. \ub2f4\uae08\uc9c8\uc774 \uc798\ubabb\ub418\uc5c8\uc744 \ub54c\uc758 \ubaa8\uc2b5\uc740 \ub2e4\uc74c\uc5d0 \ub2e4\ub8e8\uc5b4\uc838 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/quench-cracking-tool-steel\/\">\ub2f4\uae08\uc9c8 \uade0\uc5f4 \ud398\uc774\uc9c0<\/a>, \uc815\uc9c0 \uacf5\uae30 \uc911\uc5d0\uc11c \uacbd\ud654\ub418\ub294 \uac15\uc885\uc740 \ub2e4\uc74c\uc5d0\uc11c \uad6c\ubd84\ub429\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/air-hardening-tool-steel\/\">\uacf5\uae30 \uacbd\ud654 \uacf5\uad6c\uac15 \ud398\uc774\uc9c0<\/a>, \ub3d9\uc77c \uac15\uc885\uc758 \ub2e4\uc774\uce90\uc2a4\ud305 \uce21\uba74\uc740 \ub2e4\uc74c \ud398\uc774\uc9c0\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-for-die-casting-dies-inserts\/\">\ub2e4\uc774\uce90\uc2a4\ud305 \ub2e4\uc774 \ubc0f \uc778\uc11c\ud2b8 \ud398\uc774\uc9c0<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: Improved Life of Die Casting Dies of H13 Steel by Attaining Improved Mechanical Properties and Distortion Control During Heat Treatment (J. F. Wallace and D. Schwam, US Department of Energy final report DOE\/ID\/13320-3, October 1998).<\/p>","protected":false},"excerpt":{"rendered":"<p>H13 Steel Microstructure After Quenching Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, set beside the MC carbide precipitation at the austenite grain boundaries for each quench. A reference summary of published practice and not an Aobo Steel specification. What the quench decides An H13 die is [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20276","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>H13 Steel Microstructure After Quenching<\/title>\n<meta name=\"description\" content=\"Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, with the MC carbide precipitation at the austenite grain boundaries.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/h13-steel-microstructure-after-quenching\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"H13 Steel Microstructure After Quenching\" \/>\n<meta property=\"og:description\" content=\"Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, with the MC carbide precipitation at the austenite grain boundaries.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/h13-steel-microstructure-after-quenching\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:20:16+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"5\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"H13 Steel Microstructure After Quenching\",\"datePublished\":\"2026-09-29T16:13:14+00:00\",\"dateModified\":\"2026-10-15T16:20:16+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\"},\"wordCount\":1058,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\",\"name\":\"H13 Steel Microstructure After Quenching\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-29T16:13:14+00:00\",\"dateModified\":\"2026-10-15T16:20:16+00:00\",\"description\":\"Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, with the MC carbide precipitation at the austenite grain boundaries.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"H13 Steel Microstructure After Quenching\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"H13 \uac15 \ub2f4\uae08\uc9c8 \ud6c4 \ubbf8\uc138\uc870\uc9c1","description":"\uc9c4\uacf5, \uac00\uc2a4, \uc5fc\uc695, \uc720, \ud3f4\ub9ac\uba38\ub85c \ub2f4\uae08\uc9c8\ud55c H13 \ube14\ub85d\uc5d0\uc11c \uce21\uc815\ud55c \ud384\ub77c\uc774\ud2b8, \ubca0\uc774\ub098\uc774\ud2b8, \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uc640 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uacb0\uc815\ub9bd\uacc4\uc758 MC \ud0c4\ud654\ubb3c \uc11d\ucd9c\uc744 \ub2e4\ub8f9\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/h13-steel-microstructure-after-quenching\/","og_locale":"ko_KR","og_type":"article","og_title":"H13 Steel Microstructure After Quenching","og_description":"Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, with the MC carbide precipitation at the austenite grain boundaries.","og_url":"https:\/\/aobosteel.com\/ko\/h13-steel-microstructure-after-quenching\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:20:16+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"5\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"H13 Steel Microstructure After Quenching","datePublished":"2026-09-29T16:13:14+00:00","dateModified":"2026-10-15T16:20:16+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/"},"wordCount":1058,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/","url":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/","name":"H13 \uac15 \ub2f4\uae08\uc9c8 \ud6c4 \ubbf8\uc138\uc870\uc9c1","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-29T16:13:14+00:00","dateModified":"2026-10-15T16:20:16+00:00","description":"\uc9c4\uacf5, \uac00\uc2a4, \uc5fc\uc695, \uc720, \ud3f4\ub9ac\uba38\ub85c \ub2f4\uae08\uc9c8\ud55c H13 \ube14\ub85d\uc5d0\uc11c \uce21\uc815\ud55c \ud384\ub77c\uc774\ud2b8, \ubca0\uc774\ub098\uc774\ud2b8, \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uc640 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uacb0\uc815\ub9bd\uacc4\uc758 MC \ud0c4\ud654\ubb3c \uc11d\ucd9c\uc744 \ub2e4\ub8f9\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"H13 Steel Microstructure After Quenching"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"H13 Steel Microstructure After Quenching Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, set beside the MC carbide precipitation at the austenite grain boundaries for each quench. A reference summary of published practice and not an Aobo Steel specification. What the quench decides An H13 die is&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"H13 Steel Microstructure After Quenching Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, set beside the MC carbide precipitation at the austenite grain boundaries for each quench. A reference summary of published practice and not an Aobo Steel specification. What the quench decides An H13 die is&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20276","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=20276"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20276\/revisions"}],"predecessor-version":[{"id":22507,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/20276\/revisions\/22507"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=20276"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}