{"id":19812,"date":"2026-09-26T04:06:46","date_gmt":"2026-09-25T20:06:46","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=19812"},"modified":"2026-10-16T00:02:13","modified_gmt":"2026-10-15T16:02:13","slug":"m3-tool-steel-heat-treatment","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/m3-tool-steel-heat-treatment\/","title":{"rendered":"M3 \uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac"},"content":{"rendered":"<h1 class=\"wp-block-heading\">M3 \uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\ub450 \ub4f1\uae09\uc758 M3 \uace0\uc18d\ub3c4\uac15\uc5d0 \ub300\ud55c \uacbd\ud654 \uc628\ub3c4, \ub2f4\uae08\uc9c8 \ub9e4\uccb4 \ubc0f \ud15c\ud37c\ub9c1 \ubc18\uc751\uc744 \uc6d0\ubcf8 \uce74\ub4dc\uc5d0 \uac8c\uc7ac\ub41c \ub300\ub85c \uc815\ub9ac\ud588\uc2b5\ub2c8\ub2e4. \uac8c\uc7ac\ub41c \uc2e4\ubb34\uc5d0 \ub300\ud55c \ucc38\uace0 \uc694\uc57d\uc774\uba70 Aobo Steel\uc758 \uc0ac\uc591\uc774 \uc544\ub2d9\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uace0\uc18d\ub3c4\uac15 \uadf8\ub8f9\uc758 M3<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">M3\ub294 \ubab0\ub9ac\ube0c\ub374-\ud145\uc2a4\ud150 \uace0\uc18d\ub3c4\uac15\uc73c\ub85c, \uc808\uc0ad \uacf5\uad6c\uac00 \uace0\uc18d\uc5d0\uc11c \ub0a0\uc744 \uc720\uc9c0\ud558\uace0 \uadf8\uc5d0 \ub530\ub974\ub294 \uc5f4\uc744 \uacac\ub38c\uc57c \ud560 \ub54c \ud604\uc7a5\uc5d0\uc11c \uc120\ud0dd\ud558\ub294 \ub4f1\uae09\uc785\ub2c8\ub2e4. \uc6d0\ubcf8\uc740 \uc774\ub97c \ub450 \ub4f1\uae09\uc73c\ub85c \uac8c\uc7ac\ud558\uace0 \ub450 \uce74\ub4dc\ub97c M3-1\uacfc M3-2\ub85c \ud45c\uae30\ud558\uba70, \uc544\ub798 \ud45c\uc5d0\uc11c\ub3c4 \uc774 \ud45c\uae30\ub97c \uc0ac\uc6a9\ud569\ub2c8\ub2e4. \ub4f1\uae09 \uac04 \ucc28\uc774\ub294 \ud0c4\uc18c\uc640 \ubc14\ub098\ub4d0\uc5d0 \uc788\uc2b5\ub2c8\ub2e4. \ub4f1\uae09 1\uc740 \ud0c4\uc18c 1.05%\uc640 \ubc14\ub098\ub4d0 2.50%, \ub4f1\uae09 2\ub294 \ud0c4\uc18c 1.20%\uc640 \ubc14\ub098\ub4d0 3.00%\ub97c \ud568\uc720\ud558\uba70, \uac01 \ub4f1\uae09\uc740 \uace0\uc720\uc758 \uacbd\ud654 \uc628\ub3c4\uc640 \ud15c\ud37c\ub9c1 \ub77c\uc778\uc744 \uac00\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \uce74\ub4dc\ub294 \uc0ac\uc591\uc774 \uc544\ub2cc \ud604\uc7a5 \ucc38\uace0 \uc815\ubcf4\uc785\ub2c8\ub2e4. \uac01 \ub4f1\uae09\uc5d0 \ub300\ud574 \uc608\uc5f4 \ub2e8\uacc4 \ud558\ub098, \uacbd\ud654 \uc628\ub3c4 \ud558\ub098, \ub2f4\uae08\uc9c8 \ub9e4\uccb4 \ud558\ub098\ub97c \uae30\uc7ac\ud558\uace0, \uc774\uc5b4\uc11c \uac01 \ud589\uc5d0 \uacbd\ub3c4 \uc218\uce58 \ud558\ub098\uc529\ub9cc \uc788\uace0 \uc5b4\ub514\uc5d0\ub3c4 \ud5c8\uc6a9 \ubc94\uc704\uac00 \uc5c6\ub294 \ud15c\ud37c\ub9c1 \ud45c\ub97c \uac8c\uc7ac\ud569\ub2c8\ub2e4. \uc0c8 \ud788\ud2b8\uc758 \uac15\uc7ac\ub85c \ub9cc\ub4e0 \uccab \uacf5\uad6c\ub294 \uc0ac\uc774\ud074\uc744 \uc0dd\uc0b0 \uacf5\uad6c\uc5d0 \uc801\uc6a9\ud558\uae30 \uc804\uc5d0 \uc2dc\ud5d8\uc6a9\uc73c\ub85c \uac00\ub3d9\ud574 \ubcf4\ub294 \uac83\uc774 \uc88b\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">M3 \ub4f1\uae09 1 \ubc0f \ub4f1\uae09 2\uc758 \ud654\ud559 \uc131\ubd84<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">\ucc38\uace0 \uce74\ub4dc\uc5d0 \uae30\uc7ac\ub41c \uc6d0\uc18c, \ud37c\uc13c\ud2b8<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mn<\/th><th class=\"has-text-align-left\" data-align=\"left\">Si<\/th><th class=\"has-text-align-left\" data-align=\"left\">Cr<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mo<\/th><th class=\"has-text-align-left\" data-align=\"left\">V<\/th><th class=\"has-text-align-left\" data-align=\"left\">W<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">M3-1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.05<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.00<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M3-2<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.55<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.00<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, M3 \ub4f1\uae09 1 \ubc0f \ub4f1\uae09 2\uc758 \uc5f4\ucc98\ub9ac \ucc38\uace0 \uc815\ubcf4, \uc778\uc1c4 \ud398\uc774\uc9c0 190 \ubc0f 191.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uc774 \uce74\ub4dc\ub294 \uc0ac\uc591 \ubc94\uc704\uac00 \uc544\ub2cc \uac01 \uc6d0\uc18c\uc5d0 \ub300\ud574 \ud558\ub098\uc758 \uc218\uce58\ub97c \uac8c\uc7ac\ud569\ub2c8\ub2e4. \ucf54\ubc1c\ud2b8\ub294 \ub450 \ub4f1\uae09 \ubaa8\ub450\uc5d0, \ud669\uc740 \ub4f1\uae09 1\uc5d0 \uc218\uce58 \uc5c6\uc774 \ud45c\uae30\ub418\uc5b4 \uc788\uc73c\ubbc0\ub85c \ud574\ub2f9 \ud589\uc740 0\uc73c\ub85c \ud45c\uc2dc\ud558\uc9c0 \uc54a\uace0 \ud45c\uc5d0\uc11c \uc81c\uc678\ud588\uc2b5\ub2c8\ub2e4. \ud669 \uc218\uce58 \ud558\ub098\uac00 \uac8c\uc7ac\ub418\uc5b4 \uc788\ub294\ub370, \ub4f1\uae09 2 \uce74\ub4dc\uc758 0.27%\ub85c, \uace0\uc18d\ub3c4\uac15\uc5d0 \ud1b5\uc0c1 \uaddc\uc815\ub418\ub294 \ud669 \uc218\uc900\uc744 \ud6e8\uc52c \uc0c1\ud68c\ud558\ubbc0\ub85c \ud45c\uc5d0 \ubc18\uc601\ud558\uc9c0 \uc54a\uace0 \uc6d0\ubcf8\uc774 \uac8c\uc7ac\ud55c \ub300\ub85c \uc5ec\uae30\uc5d0 \uae30\ub85d\ud569\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub450 \ub4f1\uae09 \ubaa8\ub450 \ud145\uc2a4\ud150 6.00%\uc640 \ubab0\ub9ac\ube0c\ub374 5.00%, \uc774 \ub4f1\uae09\uc758 \uae30\ubc18\uc774 \ub418\ub294 \ub450 \ud0c4\ud654\ubb3c \ud615\uc131 \uc6d0\uc18c\uc640 \ud568\uaed8 \ud06c\ub86c 4.00%\ub97c \ud568\uc720\ud569\ub2c8\ub2e4. \ud0c4\uc18c\uc640 \ubc14\ub098\ub4d0\uc740 \ub4f1\uae09\uc744 \uad6c\ubd84\ud558\ub294 \ub450 \uc218\uce58\ub85c, \ub4f1\uae09 1\uc740 1.05%\uc640 2.50%, \ub4f1\uae09 2\ub294 1.20%\uc640 3.00%\uc785\ub2c8\ub2e4. \uce74\ub4dc\ub294 \ucf54\ubc1c\ud2b8\ub97c \ub450 \ub4f1\uae09 \ubaa8\ub450\uc5d0, \ud669\uc744 \ub4f1\uae09 1\uc5d0 \uc218\uce58 \uc5c6\uc774 \uae30\uc7ac\ud558\ubbc0\ub85c \ud574\ub2f9 \ud589\uc740 0\uc73c\ub85c \ud45c\uc2dc\ud558\uc9c0 \uc54a\uace0 \ud45c\uc5d0\uc11c \uc81c\uc678\ud588\uc73c\uba70, \ub4f1\uae09 2 \uce74\ub4dc\uac00 \uac8c\uc7ac\ud558\ub294 \uc720\uc77c\ud55c \ud669 \uc218\uce58\ub294 \ud45c\uc5d0 \ubc18\uc601\ud558\uc9c0 \uc54a\uace0 \ud45c \uc544\ub798\uc5d0 \uae30\ub85d\ud569\ub2c8\ub2e4. \ud45c\uc758 \uc131\ubd84 \ub370\uc774\ud130\ub294 \uc77c\ubc18 \ucc38\uace0\uc6a9\uc774\uba70, \uc2e4\uc81c \uac12\uc740 \ud45c\uc900, \uc81c\uac15\uc18c \ubc0f \ud788\ud2b8 \ubc88\ud638\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9c0\ubbc0\ub85c \ud574\ub2f9 \ud788\ud2b8\uc758 \uc7ac\ub8cc \uc2dc\ud5d8 \uc131\uc801\uc11c\uc640 \ub300\uc870\ud558\uc5ec \ud655\uc778\ud558\uac70\ub098 Aobo Steel\uc5d0 \ubb38\uc758\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">M3\uc758 \uacbd\ud654<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">\uc608\uc5f4, \uacbd\ud654 \uc628\ub3c4 \ubc0f \ub2f4\uae08\uc9c8<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uacc4<\/th><th class=\"has-text-align-left\" data-align=\"left\">M3-1<\/th><th class=\"has-text-align-left\" data-align=\"left\">M3-2<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc608\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500 \u00b0F (815 \u00b0C)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500 \u00b0F (815 \u00b0C)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">2250 \u00b0F (1230 \u00b0C)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2225 \u00b0F (1220 \u00b0C)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \ub610\ub294 \uc5fc\uc695<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \ub610\ub294 \uc5fc\uc695<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, M3 \ub4f1\uae09 1 \ubc0f \ub4f1\uae09 2\uc758 \uc5f4\ucc98\ub9ac \ucc38\uace0 \uc815\ubcf4, \uc778\uc1c4 \ud398\uc774\uc9c0 190 \ubc0f 191.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uc774 \uce74\ub4dc\ub294 \ud06c\uae30 \uc870\uac74 \uc5c6\uc774 \uc608\uc5f4 \ub2e8\uacc4 \ud558\ub098\ub97c \uac8c\uc7ac\ud558\ubbc0\ub85c, \uc774 \ub2e8\uacc4\ub294 \ub300\ud615 \ub2e8\uba74\uc5d0\ub9cc \ud544\uc694\ud55c \ub2e8\uacc4\ub85c \ud45c\uc2dc\ub418\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \ub450 \ub4f1\uae09 \ubaa8\ub450 \ub2f4\uae08\uc9c8 \ub9e4\uccb4\ub85c \uc624\uc77c \ub610\ub294 \uc5fc\uc695\uc774 \uc81c\uc2dc\ub418\uba70, \uadf8 \uc606\uc5d0 \uacf5\uae30 \ub300\uc548\uc740 \uac8c\uc7ac\ub418\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc608\uc5f4\uc740 \ub450 \uce74\ub4dc \ubaa8\ub450 1500 \u00b0F (815 \u00b0C)\uc785\ub2c8\ub2e4. \uacbd\ud654 \uc628\ub3c4\ub294 25 \u00b0F (10 \u00b0C) \ucc28\uc774\ub85c, \ub4f1\uae09 1\uc740 2250 \u00b0F (1230 \u00b0C), \ub4f1\uae09 2\ub294 2225 \u00b0F (1220 \u00b0C)\uc774\uba70, \ud569\uae08\ub7c9\uc774 \ub354 \ub9ce\uc740 \ub4f1\uae09\uc744 \uc6d0\ubcf8\uc774 \uc57d\uac04 \ub354 \ub0ae\uac8c \uc124\uc815\ud558\ub294\ub370, \uc774\ub294 \ud574\ub2f9 \ub4f1\uae09\uc744 \uad6c\ub9e4\ud558\ub294 \uc774\uc720\uc778 \ub354 \ubbf8\uc138\ud55c \uacb0\uc815\ub9bd\uc744 \uc6d0\ud560 \ub54c \ud604\uc7a5\uc5d0\uc11c \ud0dd\ud558\ub294 \ubc29\ud5a5\uc785\ub2c8\ub2e4. \ub450 \uce74\ub4dc \ubaa8\ub450 \ub2f4\uae08\uc9c8\ub85c \uc624\uc77c \ub610\ub294 \uc5fc\uc695\uc744 \uc81c\uc2dc\ud558\uace0, \uc5b4\ub290 \uce74\ub4dc\ub3c4 \uc774 \ub4f1\uae09\uc5d0 \uacf5\uae30 \ub2f4\uae08\uc9c8\uc744 \uac8c\uc7ac\ud558\uc9c0 \uc54a\uc73c\ubbc0\ub85c \ud0f1\ud06c\uc5d0\uc11c\uc758 \uc120\ud0dd\uc740 \uc624\uc77c \ub300 \uc5fc\uc695\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">M3\uc758 \ud15c\ud37c\ub9c1 \ubc18\uc751<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">\uac01 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uac00 \ub0a8\uae30\ub294 \uacbd\ub3c4<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1, \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">M3-1, HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">M3-2, HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \uc9c1\ud6c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc5c6\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">900<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><td class=\"has-text-align-left\" data-align=\"left\">63<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">950<\/td><td class=\"has-text-align-left\" data-align=\"left\">510<\/td><td class=\"has-text-align-left\" data-align=\"left\">67<\/td><td class=\"has-text-align-left\" data-align=\"left\">66<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">540<\/td><td class=\"has-text-align-left\" data-align=\"left\">67<\/td><td class=\"has-text-align-left\" data-align=\"left\">66<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1050<\/td><td class=\"has-text-align-left\" data-align=\"left\">565<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">66<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">595<\/td><td class=\"has-text-align-left\" data-align=\"left\">61<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1150<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">56<\/td><td class=\"has-text-align-left\" data-align=\"left\">63<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98, M3 \ub4f1\uae09 1 \ubc0f \ub4f1\uae09 2\uc758 \uc5f4\ucc98\ub9ac \ucc38\uace0 \uc815\ubcf4, \uc778\uc1c4 \ud398\uc774\uc9c0 190 \ubc0f 191.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uc774 \uce74\ub4dc\ub294 \ud15c\ud37c\ub9c1 \uc628\ub3c4\ub97c 900 \u00b0F\uc5d0\uc11c 1200 \u00b0F\uae4c\uc9c0 50 \u00b0F \uac04\uaca9\uc73c\ub85c \uc81c\uc2dc\ud558\uace0 \uac01 \ud589\uc5d0 \uac01 \ub4f1\uae09\uc758 \ub85c\ud06c\uc6f0 C \uc218\uce58 \ud558\ub098\ub97c \uac8c\uc7ac\ud569\ub2c8\ub2e4. \uccab \ud589\uc740 \ud15c\ud37c\ub9c1 \uc804 \ub2f4\uae08\uc9c8 \uc0c1\ud0dc\uc758 \uacbd\ub3c4\uc774\uba70, \uadf8\ub2e4\uc74c \ub450 \ud589\uc758 \uc0c1\uc2b9\uc740 2\ucc28 \uacbd\ud654\uc785\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub450 \ub4f1\uae09 \ubaa8\ub450 \ub2f4\uae08\uc9c8 \ud6c4 65 HRC\ub85c \ub098\uc624\uba70 \ub450 \ub77c\uc778 \ubaa8\ub450 \ud558\uac15\ud558\uae30 \uc804\uc5d0 \uc0c1\uc2b9\ud558\ub294\ub370, \uc774\ub294 \uccab \ud15c\ud37c\ub9c1\uc5d0 \ub530\ub974\ub294 2\ucc28 \uacbd\ud654\uc785\ub2c8\ub2e4. \ub4f1\uae09 1\uc740 950 \ubc0f 1000 \u00b0F (510 \ubc0f 540 \u00b0C)\uc5d0\uc11c 67 HRC\ub85c \uc0c1\uc2b9\ud55c \ud6c4 1200 \u00b0F (650 \u00b0C)\uc5d0\uc11c 52 HRC\ub85c \ub5a8\uc5b4\uc9d1\ub2c8\ub2e4. \ub4f1\uae09 2\ub294 \uac19\uc740 \ub450 \ud589\uc5d0\uc11c 66 HRC\ub85c \uc0c1\uc2b9\ud558\uace0 1200 \u00b0F (650 \u00b0C)\uc5d0\uc11c\ub3c4 60 HRC\ub97c \uc720\uc9c0\ud558\ub294\ub370, \uc774\ub294 \ubc94\uc704 \uc0c1\ub2e8\uc5d0\uc11c \ub4f1\uae09 1\ubcf4\ub2e4 8\ud3ec\uc778\ud2b8 \ub192\uc740 \uac12\uc785\ub2c8\ub2e4. \uace0\uc628\uc5d0\uc11c \uac00\ub3d9\ub418\uba70 \ub0a0\uc744 \uc720\uc9c0\ud574\uc57c \ud558\ub294 \uacf5\uad6c\ub294 \uc774 \uc0c1\ub2e8 \ubc94\uc704\uc5d0\uc11c \ud15c\ud37c\ub9c1\ub418\uba70, \uadf8 \uc9c0\uc810\uc5d0\uc11c \ub450 \ub77c\uc778 \uac04\uc758 \ucc28\uc774\uac00 \ub4f1\uae09 \uac04\uc758 \uc2e4\uc9c8\uc801\uc778 \ucc28\uc774\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>M3 \uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac, \uc778\uc1c4\uc6a9 PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uc774 \ud398\uc774\uc9c0\uc758 M3 \ub4f1\uae09 1 \ubc0f \ub4f1\uae09 2\uc758 \ud654\ud559 \uc131\ubd84, \uacbd\ud654 \uc0ac\uc774\ud074 \ubc0f \ud15c\ud37c\ub9c1 \ubc18\uc751\uc744 \uc5f0\ub77d\ucc98 \uc815\ubcf4\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-M3-Tool-Steel-Heat-Treatment.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 381 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ub370\uc774\ud130<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uace0\uc18d\ub3c4\uac15 \uadf8\ub8f9\uc5d0\uc11c M3 \uc606\uc5d0 \uc704\uce58\ud558\ub294 \ub4f1\uae09\ub4e4\uc740 \ub2e4\uc74c\uc5d0 \uc815\ub9ac\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/m2-tool-steel-heat-treatment\/\">M2 \uac15 \uc5f4\ucc98\ub9ac \ud398\uc774\uc9c0<\/a>, \uadf8\ub9ac\uace0 \uc774 \uadf8\ub8f9\uc774 \uad6c\ub9e4\ub418\ub294 \uc808\uc0ad \uacf5\uad6c\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/high-speed-steel-for-cutting-tools-hobs-broaches\/\">\uc808\uc0ad \uacf5\uad6c\uc6a9 \uace0\uc18d\ub3c4\uac15 \ud398\uc774\uc9c0<\/a>. \ubab0\ub9ac\ube0c\ub374 \ub4f1\uae09 \uc804\ubc18\uc758 \ud15c\ud37c\ub9c1 \ubc94\uc704\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-tempering-chart\/\">\uacf5\uad6c\uac15 \ud15c\ud37c\ub9c1 \ucc28\ud2b8<\/a>, \ubaa8\ub4e0 \uadf8\ub8f9\uc758 \uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1 \ubc94\uc704\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-hardening-tempering-chart\/\">\uacf5\uad6c\uac15 \uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1 \ucc28\ud2b8<\/a>, \uadf8\ub9ac\uace0 M \uc2dc\ub9ac\uc988\uc758 \uc131\ubd84 \ubc94\uc704\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-composition-chart\/\">\uacf5\uad6c\uac15 \uc870\uc131 \ucc28\ud2b8<\/a>. \ucf54\ubc1c\ud2b8 \ubc0f \ubab0\ub9ac\ube0c\ub374 \ub4f1\uae09\uc758 \uc7ac\uace0 \uce58\uc218\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/m42-tool-steel\/\">M42 \uacf5\uad6c\uac15 \ud398\uc774\uc9c0<\/a> \ubc0f <a href=\"https:\/\/aobosteel.com\/ko\/m35-tool-steel\/\">M35 \uacf5\uad6c\uac15 \ud398\uc774\uc9c0<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Heat Treatment, Selection, and Application of Tool Steels (William E. Bryson, \uc81c2\ud310, Hanser)\uc5d0\uc11c \ud3b8\uc9d1\ud55c \ucc38\uace0 \ub370\uc774\ud130\uc785\ub2c8\ub2e4. M3 \ub4f1\uae09 1 \ubc0f \ub4f1\uae09 2\uc758 \ud654\ud559 \uc131\ubd84, \uacbd\ud654 \uc0ac\uc774\ud074 \ubc0f \ud15c\ud37c\ub9c1 \ubc18\uc751\uc740 \uc778\uc1c4 \ud398\uc774\uc9c0 190 \ubc0f 191\uc758 \uc5f4\ucc98\ub9ac \ucc38\uace0 \uc815\ubcf4\uc5d0\uc11c \uac00\uc838\uc654\uc2b5\ub2c8\ub2e4.<\/p>","protected":false},"excerpt":{"rendered":"<p>M3 Tool Steel Heat Treatment The hardening temperature, the quench medium and the tempering response of M3 high speed steel in both classes, set out as the source card publishes it. A reference summary of published practice and not an Aobo Steel specification. M3 in the high speed group M3 is a molybdenum-tungsten high speed [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-19812","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.7 (Yoast SEO v28.7) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>M3 Tool Steel Heat Treatment and Tempering Chart<\/title>\n<meta name=\"description\" content=\"The hardening temperature, quench and tempering response of M3 high speed steel in both classes, with the chemistry and the hardness left by each temper.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/m3-tool-steel-heat-treatment\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"M3 Tool Steel Heat Treatment\" \/>\n<meta property=\"og:description\" content=\"The hardening temperature, quench and tempering response of M3 high speed steel in both classes, with the chemistry and the hardness left by each temper.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/m3-tool-steel-heat-treatment\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:02:13+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"5\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m3-tool-steel-heat-treatment\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m3-tool-steel-heat-treatment\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"M3 Tool Steel Heat Treatment\",\"datePublished\":\"2026-09-25T20:06:46+00:00\",\"dateModified\":\"2026-10-15T16:02:13+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m3-tool-steel-heat-treatment\\\/\"},\"wordCount\":997,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m3-tool-steel-heat-treatment\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/m3-tool-steel-heat-treatment\\\/\",\"name\":\"M3 Tool Steel Heat Treatment and Tempering Chart\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-25T20:06:46+00:00\",\"dateModified\":\"2026-10-15T16:02:13+00:00\",\"description\":\"The hardening temperature, quench and tempering response of M3 high speed steel in both classes, with the chemistry and the hardness left by each temper.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m3-tool-steel-heat-treatment\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/m3-tool-steel-heat-treatment\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m3-tool-steel-heat-treatment\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"M3 Tool Steel Heat Treatment\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"M3 Tool Steel Heat Treatment and Tempering Chart","description":"The hardening temperature, quench and tempering response of M3 high speed steel in both classes, with the chemistry and the hardness left by each temper.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/m3-tool-steel-heat-treatment\/","og_locale":"ko_KR","og_type":"article","og_title":"M3 Tool Steel Heat Treatment","og_description":"The hardening temperature, quench and tempering response of M3 high speed steel in both classes, with the chemistry and the hardness left by each temper.","og_url":"https:\/\/aobosteel.com\/ko\/m3-tool-steel-heat-treatment\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:02:13+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"5\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/m3-tool-steel-heat-treatment\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/m3-tool-steel-heat-treatment\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"M3 Tool Steel Heat Treatment","datePublished":"2026-09-25T20:06:46+00:00","dateModified":"2026-10-15T16:02:13+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/m3-tool-steel-heat-treatment\/"},"wordCount":997,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/m3-tool-steel-heat-treatment\/","url":"https:\/\/aobosteel.com\/m3-tool-steel-heat-treatment\/","name":"M3 Tool Steel Heat Treatment and Tempering Chart","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-25T20:06:46+00:00","dateModified":"2026-10-15T16:02:13+00:00","description":"The hardening temperature, quench and tempering response of M3 high speed steel in both classes, with the chemistry and the hardness left by each temper.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/m3-tool-steel-heat-treatment\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/m3-tool-steel-heat-treatment\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/m3-tool-steel-heat-treatment\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"M3 Tool Steel Heat Treatment"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"M3 Tool Steel Heat Treatment The hardening temperature, the quench medium and the tempering response of M3 high speed steel in both classes, set out as the source card publishes it. A reference summary of published practice and not an Aobo Steel specification. M3 in the high speed group M3 is a molybdenum-tungsten high speed&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"M3 Tool Steel Heat Treatment The hardening temperature, the quench medium and the tempering response of M3 high speed steel in both classes, set out as the source card publishes it. A reference summary of published practice and not an Aobo Steel specification. M3 in the high speed group M3 is a molybdenum-tungsten high speed&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19812","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=19812"}],"version-history":[{"count":5,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19812\/revisions"}],"predecessor-version":[{"id":22473,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19812\/revisions\/22473"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=19812"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}