{"id":19420,"date":"2026-09-21T13:28:44","date_gmt":"2026-09-21T05:28:44","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=19420"},"modified":"2026-10-16T10:31:46","modified_gmt":"2026-10-16T02:31:46","slug":"alloy-steel-composition-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/alloy-steel-composition-chart\/","title":{"rendered":"13xx~94xx \uc2dc\ub9ac\uc988 \ud569\uae08\uac15 \uc131\ubd84\ud45c"},"content":{"rendered":"<h1 id=\"h-alloy-steel-composition-chart\" class=\"wp-block-heading\">\ud569\uae08\uac15 \uc870\uc131 \ucc28\ud2b8<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">SAE-AISI \uc800\ud569\uae08 \ub4f1\uae09\uc758 \ud654\ud559 \uc870\uc131 \ud55c\ub3c4\ub85c, \uc6a9\uac15 \ub610\ub294 \uc8fc\uc870 \ubd84\uc11d \uae30\uc900 \uc911\ub7c9 \ud37c\uc13c\ud2b8\ub85c \ud45c\uae30\ub429\ub2c8\ub2e4. \ud45c\ub294 13xx \ub9dd\uac04 \uacc4\uc5f4\ubd80\ud130 40xx \ubab0\ub9ac\ube0c\ub374, 41xx \ud06c\ub86c-\ubab0\ub9ac\ube0c\ub374, 43xx~48xx \ub2c8\ucf08-\ud06c\ub86c-\ubab0\ub9ac\ube0c\ub374, 51xx \ud06c\ub86c, 61xx \ud06c\ub86c-\ubc14\ub098\ub4d0, 81xx~94xx \ubc0f 92xx \uc2e4\ub9ac\ucf58 \ub4f1\uae09\uae4c\uc9c0 \ud3ec\ud568\ud558\uba70, SAE \uc7a0\uc7ac \ud45c\uc900 PS \ub4f1\uae09\uc740 \ub450 \ubc88\uc9f8 \ud45c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>wt %<\/strong> \uc6a9\uac15 \ub610\ub294 \uc8fc\uc870 \ubd84\uc11d<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ube4c\ub9bf, \ube14\ub8f8, \uc2ac\ub798\ube0c \ubc0f \uc5f4\uac04 \uc555\uc5f0 \ub610\ub294 \ub0c9\uac04 \ub9c8\uac10 \ubd09\uac15\uc758 \uc870\uc131 \ud55c\ub3c4. \ud310\uc7ac\uc5d0\ub294 \uc57d\uac04 \ub354 \ub113\uc740 \ubc94\uc704\uac00 \uc801\uc6a9\ub429\ub2c8\ub2e4. \ucd9c\ucc98\uc758 \ud45c 19.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">SAE-AISI<\/th><th class=\"has-text-align-left\" data-align=\"left\">UNS<\/th><th class=\"has-text-align-left\" data-align=\"left\">C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mn<\/th><th class=\"has-text-align-left\" data-align=\"left\">P<\/th><th class=\"has-text-align-left\" data-align=\"left\">S<\/th><th class=\"has-text-align-left\" data-align=\"left\">Si<\/th><th class=\"has-text-align-left\" data-align=\"left\">Ni<\/th><th class=\"has-text-align-left\" data-align=\"left\">Cr<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mo<\/th><th class=\"has-text-align-left\" data-align=\"left\">V<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">1330<\/td><td class=\"has-text-align-left\" data-align=\"left\">G13300<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.28\u20130.33<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.60\u20131.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1335<\/td><td class=\"has-text-align-left\" data-align=\"left\">G13350<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.33\u20130.38<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.60\u20131.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1340<\/td><td class=\"has-text-align-left\" data-align=\"left\">G13400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.60\u20131.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1345<\/td><td class=\"has-text-align-left\" data-align=\"left\">G13450<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.43\u20130.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.60\u20131.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4023<\/td><td class=\"has-text-align-left\" data-align=\"left\">G40230<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\"><\/td><td class=\"has-text-align-left\" data-align=\"left\"><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4024<\/td><td class=\"has-text-align-left\" data-align=\"left\">G40240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035\u20130.050<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4027<\/td><td class=\"has-text-align-left\" data-align=\"left\">G40270<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4028<\/td><td class=\"has-text-align-left\" data-align=\"left\">G40280<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035\u20130.050<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4032<\/td><td class=\"has-text-align-left\" data-align=\"left\">G40320<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4037<\/td><td class=\"has-text-align-left\" data-align=\"left\">G40370<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4042<\/td><td class=\"has-text-align-left\" data-align=\"left\">G40420<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4047<\/td><td class=\"has-text-align-left\" data-align=\"left\">G40470<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4118<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41180<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4130<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41300<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.28\u20130.33<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4135<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41350<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.33\u20130.38<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4137<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41370<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"\/ko\/blog\/4140-steel-properties\/\">4140<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">G41400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4142<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41420<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4145<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41450<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.41\u20130.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4147<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41470<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4150<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41500<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.48\u20130.53<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4161<\/td><td class=\"has-text-align-left\" data-align=\"left\">G41610<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.56\u20130.64<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4320<\/td><td class=\"has-text-align-left\" data-align=\"left\">G43200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.17\u20130.22<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"\/ko\/blog\/4340-steel-properties\/\">4340<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">G43400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.60\u20130.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">E4340<sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G43406<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.65\u20130.85<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4422<\/td><td class=\"has-text-align-left\" data-align=\"left\">G44220<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35\u20130.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4427<\/td><td class=\"has-text-align-left\" data-align=\"left\">G44270<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.24\u20130.29<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35\u20130.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4615<\/td><td class=\"has-text-align-left\" data-align=\"left\">G46150<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4617<\/td><td class=\"has-text-align-left\" data-align=\"left\">G46170<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4620<\/td><td class=\"has-text-align-left\" data-align=\"left\">G46200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.17\u20130.22<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4626<\/td><td class=\"has-text-align-left\" data-align=\"left\">G46260<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.24\u20130.29<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4718<\/td><td class=\"has-text-align-left\" data-align=\"left\">G47180<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.16\u20130.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35\u20130.55<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4720<\/td><td class=\"has-text-align-left\" data-align=\"left\">G47200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.17\u20130.22<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.50\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35\u20130.55<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4815<\/td><td class=\"has-text-align-left\" data-align=\"left\">G48150<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.25\u20133.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4817<\/td><td class=\"has-text-align-left\" data-align=\"left\">G48170<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.25\u20133.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">4820<\/td><td class=\"has-text-align-left\" data-align=\"left\">G48200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.50\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.25\u20133.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50B40<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G50401<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50B44<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G50441<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.43\u20130.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5046<\/td><td class=\"has-text-align-left\" data-align=\"left\">G50460<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.43\u20130.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50B46<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G50461<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.44\u20130.49<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50B50<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G50501<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.48\u20130.53<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5060<\/td><td class=\"has-text-align-left\" data-align=\"left\">G50600<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.56\u20130.64<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50B60<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G50601<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.56\u20130.64<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5115<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51150<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5117<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51170<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5120<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.17\u20130.22<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5130<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51300<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.28\u20130.33<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5132<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51320<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.60\u20130.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5135<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51350<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.33\u20130.38<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.60\u20130.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.05<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5140<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5147<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51470<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.46\u20130.51<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.95<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.85\u20131.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5150<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51500<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.48\u20130.53<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5155<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51550<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.51\u20130.59<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5160<\/td><td class=\"has-text-align-left\" data-align=\"left\">G51600<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.56\u20130.64<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">51B60<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G51601<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.56\u20130.64<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50100<sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G50986<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.98\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">51100<sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G51986<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.98\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">52100<sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G52986<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.98\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.30\u20131.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">6118<\/td><td class=\"has-text-align-left\" data-align=\"left\">G61180<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.16\u20130.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.50\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.50\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.10\u20130.15<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">6150<\/td><td class=\"has-text-align-left\" data-align=\"left\">G61500<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.48\u20130.53<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15 min<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8115<\/td><td class=\"has-text-align-left\" data-align=\"left\">G81150<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">81B45<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G81451<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.43\u20130.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35\u20130.55<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8615<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86150<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8617<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86170<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8620<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8622<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86220<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8625<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86250<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.23\u20130.28<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8627<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86270<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8630<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86300<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.28\u20130.33<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8637<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86370<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"\/ko\/blog\/8620-steel-properties\/\">8640<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">G86400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8642<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86420<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8645<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86450<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.43\u20130.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">86B45<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G86451<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.43\u20130.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8650<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86500<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.48\u20130.53<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8655<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86550<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.51\u20130.59<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8600<\/td><td class=\"has-text-align-left\" data-align=\"left\">G86600<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.56\u20130.64<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8720<\/td><td class=\"has-text-align-left\" data-align=\"left\">G87200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8740<\/td><td class=\"has-text-align-left\" data-align=\"left\">G87400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8822<\/td><td class=\"has-text-align-left\" data-align=\"left\">G88220<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">9254<\/td><td class=\"has-text-align-left\" data-align=\"left\">G92540<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.51\u20130.59<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.60\u20130.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.20\u20131.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.60\u20130.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">9260<\/td><td class=\"has-text-align-left\" data-align=\"left\">G92600<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.56\u20130.64<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.80\u20132.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">9310<sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G93106<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.13<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.00\u20133.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00\u20131.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">94B15<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G94151<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">94B17<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G94171<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">94B30<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">G94301<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.28\u20130.33<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30\u20130.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Vol 1 (10th ed.), &#8220;Classification and Designation of Carbon and Low-Alloy Steels&#8221;, Table 19.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\ud569\uae08\uac15 \ud654\ud559 \uc131\ubd84\ud45c, \uc778\uc1c4\uc6a9 PDF<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">116\uac1c \uac15\uc885\uc758 \ud654\ud559 \uc131\ubd84 \ud55c\uacc4, \ub9dd\uac00\ub2c8\uc988, \ubab0\ub9ac\ube0c\ub374, \ud06c\ub86c, \ub2c8\ucf08 \uacc4\uc5f4\uacfc SAE PS \uac15\uc885, \uc6d0\ubb38 \uc8fc\uc11d\uc5d0 \ud45c\uc2dc\ub41c \uac12, \uc5f0\ub77d\ucc98\ub97c \ub2f4\uc740 A4 3\ud398\uc774\uc9c0\uc785\ub2c8\ub2e4. PDF\ub294 \uc601\uc5b4\ub85c \uc81c\uacf5\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Alloy-Steel-Composition-Chart.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 798 KB<\/a><\/div>\n<\/div>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">SAE \uc7a0\uc7ac \ud45c\uc900\uac15<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">PS \uc2dc\ub9ac\uc988\ub294 \ud45c\uc900\uc73c\ub85c \uc81c\uc548\ub41c \ub4f1\uae09\uc73c\ub85c, \ud654\ud559 \uc131\ubd84\ub9cc\uc774 \uc544\ub2c8\ub77c \uacbd\ud654\ub2a5 \uc694\uad6c \uc0ac\ud56d\uc5d0 \ub530\ub77c \uacf5\uae09\ub418\ub294 \uacbd\uc6b0\uac00 \ub9ce\uc2b5\ub2c8\ub2e4. \ucd9c\ucc98\uc758 Table 20.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">SAE PS \ubc88\ud638<\/th><th class=\"has-text-align-left\" data-align=\"left\">C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mn<\/th><th class=\"has-text-align-left\" data-align=\"left\">P \ucd5c\ub300<\/th><th class=\"has-text-align-left\" data-align=\"left\">S \ucd5c\ub300<\/th><th class=\"has-text-align-left\" data-align=\"left\">Si<\/th><th class=\"has-text-align-left\" data-align=\"left\">Ni<\/th><th class=\"has-text-align-left\" data-align=\"left\">Cr<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mo<\/th><th class=\"has-text-align-left\" data-align=\"left\">B<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.19\u20130.24<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.95\u20131.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05\u20130.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 15<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 16<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 17<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.23\u20130.28<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 19<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0005\u20130.003<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 21<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 24<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20\u20130.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 31<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 32<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 33<sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">0.17\u20130.24<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.85\u20131.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 34<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.28\u20130.33<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.60<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 36<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.38\u20130.43<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 38<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.43\u20130.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 39<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.48\u20130.53<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 40<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.51\u20130.59<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 54<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.19\u20130.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20131.05<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 55<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.65\u20130.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 56<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.080\u20130.13<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20131.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.445\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.65\u20130.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 57<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25 max<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.00\u201319.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.75\u20132.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 58<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.16\u20130.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00\u20131.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 59<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.18\u20130.23<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00\u20131.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 61<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.23\u20130.28<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00\u20131.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 63<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.31\u20130.38<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75\u20131.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.65<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0005\u20130.003<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 64<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.16\u20130.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00\u20131.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 65<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.21\u20130.26<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00\u20131.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70\u20130.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 66<sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">0.16\u20130.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40\u20130.70<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.65\u20132.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.45\u20130.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08\u20130.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PS 67<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.42\u20130.49<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.80\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.85\u20131.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25\u20130.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Vol 1 (10th ed.), &#8220;Classification and Designation of Carbon and Low-Alloy Steels&#8221;, Table 20.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\ud569\uae08\uac15 \ud654\ud559 \uc131\ubd84\ud45c, \uc778\uc1c4\uc6a9 PDF<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">116\uac1c \uac15\uc885\uc758 \ud654\ud559 \uc131\ubd84 \ud55c\uacc4, \ub9dd\uac00\ub2c8\uc988, \ubab0\ub9ac\ube0c\ub374, \ud06c\ub86c, \ub2c8\ucf08 \uacc4\uc5f4\uacfc SAE PS \uac15\uc885, \uc6d0\ubb38 \uc8fc\uc11d\uc5d0 \ud45c\uc2dc\ub41c \uac12, \uc5f0\ub77d\ucc98\ub97c \ub2f4\uc740 A4 3\ud398\uc774\uc9c0\uc785\ub2c8\ub2e4. PDF\ub294 \uc601\uc5b4\ub85c \uc81c\uacf5\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Alloy-Steel-Composition-Chart.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 798 KB<\/a><\/div>\n<\/div>\n<\/div>\n\n\n\n<ul class=\"wp-block-list\">\n<li><sup>(a)<\/sup> \ud569\uae08\uac15\uc5d0\ub294 \uaddc\uc815\ub418\uac70\ub098 \uc694\uad6c\ub418\uc9c0 \uc54a\uc740 \ud2b9\uc815 \uc6d0\uc18c\uac00 \uc18c\ub7c9 \ud568\uc720\ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc774\ub7ec\ud55c \uc6d0\uc18c\ub294 \ubd80\uc218\uc801\uc778 \uac83\uc73c\ub85c \uac04\uc8fc\ub418\uba70 \ub2e4\uc74c \ucd5c\ub300\uce58\uae4c\uc9c0 \ud5c8\uc6a9\ub429\ub2c8\ub2e4. \uad6c\ub9ac 0.35%, \ub2c8\ucf08 0.25%, \ud06c\ub86c 0.20%, \ubab0\ub9ac\ube0c\ub374 0.06%.<\/li>\n\n\n\n<li><sup>(b)<\/sup> \uc804\uae30\ub85c\uac15\uc774\ubbc0\ub85c E4340 \ud589\uc740 \uc704\uc758 4340 \ud589\ubcf4\ub2e4 \uc778\uacfc \ud669 \ud568\ub7c9\uc774 \ub0ae\uc2b5\ub2c8\ub2e4.<\/li>\n\n\n\n<li><sup>(c)<\/sup> \ubd95\uc18c \ud568\ub7c9\uc740 0.0005-0.003%\uc785\ub2c8\ub2e4. \ubd95\uc18c\ub294 \ud569\uae08 \ud568\ub7c9\uc758 \uc77c\ubd80\ub97c \ub300\uccb4\ud558\uc5ec \uacbd\ud654\ub2a5\uc744 \ub192\uc774\uae30 \uc704\ud574 \ucca8\uac00\ub418\uba70, \ubb38\uc790 B\ub294 \ub4f1\uae09 \ubc88\ud638\uc758 \ub9c8\uc9c0\ub9c9 \ub450 \uc790\ub9ac \uc55e\uc5d0 \uc704\uce58\ud569\ub2c8\ub2e4.<\/li>\n\n\n\n<li><sup>(d)<\/sup> \uc77c\ubd80 PS \uac15\uc740 \uacbd\ud654\ub2a5 \uc694\uad6c \uc0ac\ud56d\uc5d0 \ub530\ub77c \uacf5\uae09\ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4. PS 34\uc640 PS 38\uc740 J4\uc5d0\uc11c 23-43 HRC \ubc94\uc704 \ub0b4 15 HRC \ud3ec\uc778\ud2b8\uc758 \uacbd\ud654\ub2a5 \uc694\uad6c \uc0ac\ud56d\uc73c\ub85c \uacf5\uae09\ub418\uba70, PS 66\uc740 \ubc14\ub098\ub4d0 \ud568\ub7c9\uc774 0.10-0.15%\uc785\ub2c8\ub2e4.<\/li>\n<\/ul>\n\n\n\n<h3 id=\"h-table-notes\" class=\"wp-block-heading\">\ud14c\uc774\ube14 \ub178\ud2b8<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\uc6d0\ubcf8 \ud45c\uc758 \uc138 \uac00\uc9c0 \uac12\uc740 \uacb0\ud568\uc774 \uc788\ub294 \uc0c1\ud0dc\ub85c \uc778\uc1c4\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. \ub4f1\uae09 4118\uc758 \ubab0\ub9ac\ube0c\ub374\uc740 0.08-015\ub85c \uc778\uc1c4\ub418\uc5b4 \uc788\uc73c\uba70 \uc5ec\uae30\uc11c\ub294 0.08-0.15\ub85c \ud45c\uae30\ud569\ub2c8\ub2e4. 15% \ubab0\ub9ac\ube0c\ub374 \ubc94\uc704\ub294 \ubd88\uac00\ub2a5\ud558\uace0 \ub3d9\uc77c\ud55c \ud654\ud559 \uc870\uc131\uc774 \ud45c\uc758 \ub2e4\ub978 \uacf3\uc5d0\uc11c 4118\ud615 \ub4f1\uae09\uc5d0 \ub300\ud574 \uc62c\ubc14\ub974\uac8c \uc778\uc1c4\ub418\uc5b4 \uc788\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \ub4f1\uae09 4023\uc740 \ub2e4\ub978 \ubaa8\ub4e0 \ud589\uc774 \ubbf8\uaddc\uc815 \ud45c\uc2dc\ub97c \uac00\uc9c0\uace0 \uc788\ub294 \ubc18\uba74 \ubab0\ub9ac\ube0c\ub374 \uc140\uacfc \ubc14\ub098\ub4d0 \uc140\uc774 \ube44\uc5b4 \uc788\uc73c\uba70, \ud574\ub2f9 \ud589\uc740 \uc778\uc1c4\ub41c \uadf8\ub300\ub85c \uc7ac\ud604\ub429\ub2c8\ub2e4. \ub4f1\uae09 8600\uc740 SAE 8660\uc5d0 \uc18d\ud558\ub294 UNS \ubc88\ud638 G86600\uc5d0 \ub300\ud574 \uc778\uc1c4\ub418\uc5b4 \uc788\uc73c\uba70, \ud574\ub2f9 \ud589\uc740 \ubc88\ud638\ub97c \ub2e4\uc2dc \ub9e4\uae30\uc9c0 \uc54a\uace0 \uc778\uc1c4\ub41c \uadf8\ub300\ub85c \uc7ac\ud604\ub429\ub2c8\ub2e4. \ub450 \uac00\uc9c0 \ucd94\uac00 \uac12\uc740 \uc6d0\ubcf8\uc774 \uc778\uc1c4\ud55c \uadf8\ub300\ub85c \uc7ac\ud604\ub418\uc5c8\uc73c\uba70 \ud2b9\uc774\ud574 \ubcf4\uc785\ub2c8\ub2e4. PS 56\uc740 0.080-0.13% C\uc640 0.445-0.65% Cr\uc744 \uac00\uc9c0\uba70, PS 57\uc740 S max\ub77c\ub294 \uc5f4 \uc81c\ubaa9 \uc544\ub798\uc5d0 0.15-0.35% \ud669\uc744 \uac00\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc704 \uac12\uc740 \uc911\ub7c9 \ud37c\uc13c\ud2b8 \uae30\uc900 \ub808\uc774\ub4e4 \ub610\ub294 \uc8fc\uc870 \ubd84\uc11d \ud55c\uacc4\uc785\ub2c8\ub2e4. \uc81c\ud488 \ubd84\uc11d \uacf5\ucc28\ub294 \ub354 \ub113\uc73c\uba70 \uc801\uc6a9 \ud45c\uc900\uc5d0 \uc758\ud574 \uc124\uc815\ub429\ub2c8\ub2e4. \ud788\ud2b8\ub97c \ucd9c\ud558\ud558\uae30 \uc804\uc5d0 \uc8fc\ubb38\uc5d0 \uc801\uc6a9\ub418\ub294 \ud55c\uacc4\ub97c \uc7ac\ub8cc \uc2dc\ud5d8 \uc131\uc801\uc11c \ub610\ub294 \uc544\uc624\ubcf4 \uc2a4\ud2f8\uacfc \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc870\uc131 \ub370\uc774\ud130\ub294 \uc77c\ubc18 \ucc38\uace0\uc6a9\uc785\ub2c8\ub2e4. \uc2e4\uc81c \uac12\uc740 \ud45c\uc900, \uc81c\ucca0\uc18c \ubc0f \ud788\ud2b8 \ubc88\ud638\uc5d0 \ub530\ub77c \ub2e4\ub985\ub2c8\ub2e4. \uc7ac\ub8cc \uc2dc\ud5d8 \uc131\uc801\uc11c(MTC)\uc640 \ud655\uc778\ud558\uac70\ub098 \uc544\uc624\ubcf4 \uc2a4\ud2f8\uc5d0 \ubb38\uc758\ud558\uc2ed\uc2dc\uc624. \uac1c\ubcc4 \uac15\uc885\uc5d0 \ub300\ud55c \ub4f1\uae09 \ud398\uc774\uc9c0(\uc608: <a href=\"\/ko\/blog\/4140-steel-properties\/\">4140 \uc870\uc131<\/a>\ub294 \ud558\ub098\uc758 \ub4f1\uae09\uc5d0 \ub300\ud574 \ub3d9\uc77c\ud55c \ud45c \uac12\uc744 \uc5f4\ucc98\ub9ac \ubc0f \uc751\uc6a9 \ubd84\uc57c\uc640 \ud568\uaed8 \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 id=\"h-why-the-same-grade-has-two-chemistries\" class=\"wp-block-heading\">\ub3d9\uc77c \ub4f1\uae09\uc5d0 \ub450 \uac00\uc9c0 \ud654\ud559 \uc870\uc131\uc774 \uc788\ub294 \uc774\uc720<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc704\uc758 4340 \ud589\uc740 0.035% \uc778\uacfc 0.040% \ud669\uc744 \uac00\uc9d1\ub2c8\ub2e4. \uc544\ub798\uc758 E4340 \ud589\uc740 0.025\uc640 0.025\ub97c \uac00\uc9c0\ub294\ub370, E\ub294 \ub354 \uae68\ub057\ud55c \uc794\ub958 \uc218\uc900\uc758 \uc804\uae30\ub85c\uac15\uc744 \ub098\ud0c0\ub0b4\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \ub458 \ub2e4 \ub4f1\uae09 \ubc88\ud638\uc5d0 \ub300\ud574 \uc815\ud655\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 id=\"h-boron-saves-alloy-content\" class=\"wp-block-heading\">\ubd95\uc18c\ub294 \ud569\uae08 \ud568\ub7c9\uc744 \uc808\uc57d\ud569\ub2c8\ub2e4<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ubd95\uc18c \ub4f1\uae09\uc740 \ub354 \uc801\uc740 \ub2c8\ucf08, \ud06c\ub86c \ubc0f \ubab0\ub9ac\ube0c\ub374\uc73c\ub85c \ub3d9\uc77c\ud55c \uacbd\ud654\ub2a5\uc5d0 \ub3c4\ub2ec\ud569\ub2c8\ub2e4. <a href=\"\/ko\/blog\/case-hardening-steel-guide\/\">\uce68\ud0c4\uac15 \uac00\uc774\ub4dc<\/a> \ub294 \uce68\ud0c4 \ubd80\ud488\uc5d0\uc11c \uadf8 \uac70\ub798\uac00 \uac00\uce58\uac00 \uc788\ub294 \uc2dc\uc810\uc744 \uc81c\uc2dc\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 id=\"h-chromium-and-molybdenum-do-the-work\" class=\"wp-block-heading\">\ud06c\ub86c\uacfc \ubab0\ub9ac\ube0c\ub374\uc774 \uc5ed\ud560\uc744 \ud569\ub2c8\ub2e4<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">41xx \uacc4\uc5f4\uc5d0\uc11c \ud06c\ub86c\uc740 \uacbd\ud654\ub2a5\uc744 \ub2f4\ub2f9\ud558\uace0 \ubab0\ub9ac\ube0c\ub374\uc740 \ub728\uc784 \uc800\ud56d\uc131\uc744 \ub2f4\ub2f9\ud569\ub2c8\ub2e4. <a href=\"\/ko\/blog\/4140-steel-properties\/\">4140 \ud2b9\uc131 \ud398\uc774\uc9c0<\/a> \ub294 \uadf8 \uc870\ud569\uc774 \uacbd\ub3c4\uc640 \uc5f4\ucc98\ub9ac\uc5d0 \ubbf8\uce58\ub294 \uc601\ud5a5\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 id=\"h-ask-for-the-certificate-with-the-heat-number\" class=\"wp-block-heading\">\ud788\ud2b8 \ubc88\ud638\uac00 \uae30\uc7ac\ub41c \uc778\uc99d\uc11c\ub97c \uc694\uccad\ud558\uc2ed\uc2dc\uc624<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ubaa8\ub4e0 \ud569\uae08\uac15 \ucd9c\ud558\ud488\uc5d0\ub294 \ud788\ud2b8 \ubc88\ud638\uac00 \ud3ec\ud568\ub41c EN 10204 3.1 \ubc00 \uc778\uc99d\uc11c\uac00 \ud568\uaed8 \uc81c\uacf5\ub418\ubbc0\ub85c, \uc704\uc758 \ud55c\uacc4\uac12\uc744 \uc2e4\uc81c\ub85c \uc555\uc5f0\ub41c \ud788\ud2b8\uc640 \ub300\uc870\ud558\uc5ec \ud655\uc778\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 id=\"h-related-reference-pages\" class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ud398\uc774\uc9c0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"\/ko\/carbon-steel-composition-chart\/\">\ud0c4\uc18c\uac15 \uc870\uc131 \ucc28\ud2b8<\/a> \u00b7 <a href=\"\/ko\/tool-steel-composition-chart\/\">\uacf5\uad6c\uac15 \uad6c\uc131\ud45c<\/a> \u00b7 <a href=\"\/ko\/stainless-steel-composition-chart\/\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uc131\ubd84\ud45c<\/a> \u00b7 <a href=\"\/ko\/blog\/4140-steel-properties\/\">4140 \uac15\uc7ac \ud2b9\uc131<\/a> \u00b7 <a href=\"\/ko\/blog\/4340-steel-properties\/\">4340 \uac15\uc7ac \ud2b9\uc131<\/a> \u00b7 <a href=\"\/ko\/blog\/8620-steel-properties\/\">8620 \uac15\uc7ac \ud2b9\uc131<\/a> \u00b7 <a href=\"\/ko\/blog\/case-hardening-steel-guide\/\">\uce68\ud0c4\uac15 \uac00\uc774\ub4dc<\/a> \u00b7 <a href=\"\/ko\/scm415-alloy-steel\/\">SCM415 \ud569\uae08\uac15<\/a> \u00b7 <a href=\"\/ko\/steel-machinability-ratings-chart\/\">\uac15\ucca0 \ud53c\uc0ad\uc131 \ub4f1\uae09<\/a> \u00b7 <a href=\"\/ko\/h-steel-composition-chart\/\">H \uac15\ucca0 \uc870\uc131 \ucc28\ud2b8<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Vol 1 (10th ed.), &#8220;Classification and Designation of Carbon and Low-Alloy Steels&#8221;, Tables 19 and 20. \uac12\uc740 \uc911\ub7c9 \ud37c\uc13c\ud2b8 \uae30\uc900 \ub808\uc774\ub4e4 \ub610\ub294 \uc8fc\uc870 \ubd84\uc11d \ud55c\uacc4\uc785\ub2c8\ub2e4.<\/p>","protected":false},"excerpt":{"rendered":"<p>Alloy Steel Composition Chart Chemical composition limits for the SAE-AISI low-alloy grades, quoted as ladle or cast analysis in weight percent. The table runs from the 13xx manganese series through the 40xx molybdenum, 41xx chromium-molybdenum, 43xx to 48xx nickel-chromium-molybdenum, 51xx chromium, 61xx chromium-vanadium, 81xx to 94xx and 92xx silicon grades, with the SAE potential standard [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-19420","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Alloy Steel Composition Chart, 13xx to 94xx | Aobo Steel<\/title>\n<meta name=\"description\" content=\"Ladle composition limits for 116 SAE-AISI low-alloy steel grades from the 13xx to the 94xx series, with the SAE potential standard PS grades in a second table.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/alloy-steel-composition-chart\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Alloy Steel Composition Chart for the 13xx to 94xx Series\" \/>\n<meta property=\"og:description\" content=\"Ladle composition limits for 116 SAE-AISI low-alloy steel grades from the 13xx to the 94xx series, with the SAE potential standard PS grades in a second table.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/alloy-steel-composition-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-16T02:31:46+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"9\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/alloy-steel-composition-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/alloy-steel-composition-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Alloy Steel Composition Chart for the 13xx to 94xx Series\",\"datePublished\":\"2026-09-21T05:28:44+00:00\",\"dateModified\":\"2026-10-16T02:31:46+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/alloy-steel-composition-chart\\\/\"},\"wordCount\":986,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/alloy-steel-composition-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/alloy-steel-composition-chart\\\/\",\"name\":\"Alloy Steel Composition Chart, 13xx to 94xx | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-21T05:28:44+00:00\",\"dateModified\":\"2026-10-16T02:31:46+00:00\",\"description\":\"Ladle composition limits for 116 SAE-AISI low-alloy steel grades from the 13xx to the 94xx series, with the SAE potential standard PS grades in a second table.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/alloy-steel-composition-chart\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/alloy-steel-composition-chart\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/alloy-steel-composition-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Alloy Steel Composition Chart for the 13xx to 94xx Series\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\ud569\uae08\uac15 \uc131\ubd84 \ucc28\ud2b8, 13xx~94xx | Aobo Steel","description":"13xx\ubd80\ud130 94xx \uacc4\uc5f4\uae4c\uc9c0 116\uac1c SAE-AISI \uc800\ud569\uae08\uac15 \ub4f1\uae09\uc758 \uc6a9\uac15 \uc870\uc131 \ud55c\ub3c4. SAE \uc7a0\uc7ac \ud45c\uc900 PS \ub4f1\uae09\uc740 \ub450 \ubc88\uc9f8 \ud45c\uc5d0 \uc218\ub85d.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/alloy-steel-composition-chart\/","og_locale":"ko_KR","og_type":"article","og_title":"Alloy Steel Composition Chart for the 13xx to 94xx Series","og_description":"Ladle composition limits for 116 SAE-AISI low-alloy steel grades from the 13xx to the 94xx series, with the SAE potential standard PS grades in a second table.","og_url":"https:\/\/aobosteel.com\/ko\/alloy-steel-composition-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-16T02:31:46+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"9\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/alloy-steel-composition-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/alloy-steel-composition-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Alloy Steel Composition Chart for the 13xx to 94xx Series","datePublished":"2026-09-21T05:28:44+00:00","dateModified":"2026-10-16T02:31:46+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/alloy-steel-composition-chart\/"},"wordCount":986,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/alloy-steel-composition-chart\/","url":"https:\/\/aobosteel.com\/alloy-steel-composition-chart\/","name":"\ud569\uae08\uac15 \uc131\ubd84 \ucc28\ud2b8, 13xx~94xx | Aobo Steel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-21T05:28:44+00:00","dateModified":"2026-10-16T02:31:46+00:00","description":"13xx\ubd80\ud130 94xx \uacc4\uc5f4\uae4c\uc9c0 116\uac1c SAE-AISI \uc800\ud569\uae08\uac15 \ub4f1\uae09\uc758 \uc6a9\uac15 \uc870\uc131 \ud55c\ub3c4. SAE \uc7a0\uc7ac \ud45c\uc900 PS \ub4f1\uae09\uc740 \ub450 \ubc88\uc9f8 \ud45c\uc5d0 \uc218\ub85d.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/alloy-steel-composition-chart\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/alloy-steel-composition-chart\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/alloy-steel-composition-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Alloy Steel Composition Chart for the 13xx to 94xx Series"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Alloy Steel Composition Chart Chemical composition limits for the SAE-AISI low-alloy grades, quoted as ladle or cast analysis in weight percent. The table runs from the 13xx manganese series through the 40xx molybdenum, 41xx chromium-molybdenum, 43xx to 48xx nickel-chromium-molybdenum, 51xx chromium, 61xx chromium-vanadium, 81xx to 94xx and 92xx silicon grades, with the SAE potential standard&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Alloy Steel Composition Chart Chemical composition limits for the SAE-AISI low-alloy grades, quoted as ladle or cast analysis in weight percent. The table runs from the 13xx manganese series through the 40xx molybdenum, 41xx chromium-molybdenum, 43xx to 48xx nickel-chromium-molybdenum, 51xx chromium, 61xx chromium-vanadium, 81xx to 94xx and 92xx silicon grades, with the SAE potential standard&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19420","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=19420"}],"version-history":[{"count":8,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19420\/revisions"}],"predecessor-version":[{"id":23043,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19420\/revisions\/23043"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=19420"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}