{"id":19287,"date":"2026-09-19T07:33:13","date_gmt":"2026-09-18T23:33:13","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=19287"},"modified":"2026-10-22T12:10:48","modified_gmt":"2026-10-22T04:10:48","slug":"hardness-test-correction-factors-round-bar","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/hardness-test-correction-factors-round-bar\/","title":{"rendered":"\ud658\ubd09\uc6a9 \uacbd\ub3c4 \uc2dc\ud5d8 \ubcf4\uc815 \uacc4\uc218"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\ud658\ubd09\uc6a9 \uacbd\ub3c4 \uc2dc\ud5d8 \ubcf4\uc815 \uacc4\uc218<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\ud658\ubd09\uc5d0\uc11c \uce21\uc815\ud55c \uacbd\ub3c4 \uac12\uc740 \ub3d9\uc77c\ud55c \uc7ac\uc9c8\uc758 \ud3c9\uac15\uc5d0\uc11c \uce21\uc815\ud55c \uac12\uacfc \ub3d9\uc77c\ud558\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \uc774 \ud398\uc774\uc9c0\ub294 \ub85c\ud06c\uc6f0 \uc2a4\ucf00\uc77c\uc5d0\uc11c \uc6d0\ud1b5\ud615 \uacf5\uc791\ubb3c\uc5d0 \ub300\ud55c \uacf5\uac1c\ub41c \ubcf4\uc815 \uacc4\uc218\ub97c \uc218\ub85d\ud558\uace0 \uc788\uc73c\uba70, \ubcf4\uc815\uc774 \ud544\uc694\ud55c \uc2dc\uc810\uc744 \uacb0\uc815\ud558\ub294 \uc9c1\uacbd \ud55c\uacc4\ub97c \uc81c\uc2dc\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uace1\uba74\uc5d0\uc11c \ub0ae\uac8c \uce21\uc815\ub418\ub294 \uc774\uc720<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uace1\uba74\uc5d0\uc11c \ub0ae\uac8c \uce21\uc815\ub418\ub294 \uc774\uc720<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ubcf4\uc815 \uac12\uc740 \ubcfc\ub85d\ud55c \ud45c\uba74\uc5d0\uc11c\ub294 \uce21\uc815\uac12\uc5d0 \ub354\ud558\uace0 \uc624\ubaa9\ud55c \ud45c\uba74\uc5d0\uc11c\ub294 \ube8d\ub2c8\ub2e4. \uacf5\uac1c\ub41c \uac12\uc740 \uc5ec\ub7ec \uc2e4\ud5d8\uc2e4\uc758 \uce21\uc815\uac12\uacfc \ub3d9\uc77c \ubb38\uc81c\uc5d0 \ub300\ud55c \ubd84\uc11d\uc5d0\uc11c \uc5bb\uc740 \uac83\uc73c\ub85c, \uac00\uc7a5 \uac00\uae4c\uc6b4 0.5 \ub85c\ud06c\uc6f0 \uc218\uce58\ub85c \ubc18\uc62c\ub9bc\ud55c \ud3c9\uade0\uac12\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc9c1\uacbd 25 mm(1 in.) \uc774\uc0c1\uc5d0\uc11c\ub294 \ub85c\ud06c\uc6f0 \uc2a4\ucf00\uc77c\uc5d0\uc11c \ucc28\uc774\uac00 \ubb34\uc2dc\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uadf8 \uc774\ud558\uc758 \uc9c1\uacbd, \ud2b9\ud788 \uc555\uc785\uc774 \ub354 \ud070 \uc5f0\uc9c8 \uc7ac\ub8cc\uc5d0\uc11c\ub294 \uac12\uc744 \ud3c9\uba74 \ub610\ub294 \ub2e4\ub978 \uc9c1\uacbd\uacfc \ube44\uad50\ud558\uae30 \uc804\uc5d0 \uace1\ub960\uc744 \ubcf4\uc815\ud574\uc57c \ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc77c\ubc18 \ub85c\ud06c\uc6f0 \uc2a4\ucf00\uc77c\uc740 \uc9c1\uacbd 6.35 mm(0.25 in.)\uae4c\uc9c0\uc758 \uc6d0\ud1b5\uc5d0 \uc0ac\uc6a9\ud560 \uc218 \uc788\uc73c\uba70, \uc774\uac83\uc774 C, D \ubc0f A \uc2a4\ucf00\uc77c\uc5d0\uc11c 3.175 mm \uc5f4\uc774 \ube44\uc5b4 \uc788\ub294 \uc774\uc720\uc785\ub2c8\ub2e4. \ud45c\uba74 \ub85c\ud06c\uc6f0 \ubcf4\uc815 \uac12\uc740 3.175 mm(0.125 in.)\uae4c\uc9c0 \uc801\uc6a9\ub418\uba70, \uadf8 \uc774\ud558\uc758 \uc9c1\uacbd\uc740 \ubbf8\uc138 \uc555\uc785 \ubc29\ubc95\uc5d0 \ud574\ub2f9\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uace1\uba74\uc5d0\uc11c \uce21\uc815\ud55c \uacb0\uacfc\ub294 \uace1\ub960 \ubc18\uacbd \uc5c6\uc774 \ubcf4\uace0\ud574\uc11c\ub294 \uc548 \ub429\ub2c8\ub2e4. \uc6d0\ud1b5\ud615 \uacf5\uc791\ubb3c\uc758 \uc815\ud655\ub3c4\ub294 \uc2b9\uac15 \ub098\uc0ac, V\ud615 \uc564\ube4c \ubc0f \uc555\uc785\uc790\uc758 \uc815\ub82c\uacfc \ubd09\uc7ac\uc758 \ud45c\uba74 \uc870\ub3c4 \ubc0f \uc9c1\uc9c4\ub3c4\uc5d0\ub3c4 \ub2ec\ub824 \uc788\uc2b5\ub2c8\ub2e4. \ube0c\ub9ac\ub12c \uc2dc\ud5d8\uc758 \uacbd\uc6b0 \uace1\ub960 \ubc18\uacbd\uc774 \uc555\uc785\uc790 \ubcfc \uc9c1\uacbd\uc758 2.5\ubc30\ubcf4\ub2e4 \ucee4\uc57c \ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc6d0\ud1b5\ud615 \uacf5\uc791\ubb3c\uc6a9 \ubcf4\uc815 \uacc4\uc218, \ud45c\uc900 \ub85c\ud06c\uc6f0<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc6d0\ud1b5\uc758 \uc678\ubd80 \ud45c\uba74\uc5d0\uc11c\ub294 \uac12\uc744 \ub354\ud558\uace0 \ub0b4\ubd80 \ud45c\uba74\uc5d0\uc11c\ub294 \ube8d\ub2c8\ub2e4. \uc5f4\uc740 \uacf5\uc791\ubb3c \uc9c1\uacbd\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2e4\uc774\uc544\ubaac\ub4dc \uc555\uc785\uc790, \ub85c\ud06c\uc6f0 C, D \ubc0f A \uc2a4\ucf00\uc77c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uce21\uc815\uac12<\/th><th class=\"has-text-align-left\" data-align=\"left\">3.175<br>0.125 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">6.350<br>0.250 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">9.525<br>0.375 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">12.700<br>0.500 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">15.875<br>0.625 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">19.050<br>0.750 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">22.225<br>0.875 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">25.400<br>1.000 in.<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">1.588 mm(1\/16 in.) \ubcfc \uc555\uc785\uc790, \ub85c\ud06c\uc6f0 B, F \ubc0f G \uc2a4\ucf00\uc77c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uce21\uc815\uac12<\/th><th class=\"has-text-align-left\" data-align=\"left\">3.175<br>0.125 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">6.350<br>0.250 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">9.525<br>0.375 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">12.700<br>0.500 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">15.875<br>0.625 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">19.050<br>0.750 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">22.225<br>0.875 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">25.400<br>1.000 in.<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98: ASM Handbook, Vol. 8, \ud45c\uc900 \ub85c\ud06c\uc6f0 \uacbd\ub3c4 \uc2dc\ud5d8\uae30\ub85c \uc2dc\ud5d8\ud55c \uc6d0\ud1b5\ud615 \uacf5\uc791\ubb3c\uc758 \ubcf4\uc815 \uacc4\uc218.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc6d0\ud1b5\ud615 \uacf5\uc791\ubb3c\uc6a9 \ubcf4\uc815 \uacc4\uc218, \ud45c\uba74 \ub85c\ud06c\uc6f0<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud45c\uba74 \ub85c\ud06c\uc6f0 \uc2a4\ucf00\uc77c\uc740 \uc77c\ubc18 \uc2a4\ucf00\uc77c\uc774 \ubd80\ud488\uc5d0 \ub108\ubb34 \ubb34\uac70\uc6b4 \uc587\uc740 \ub2e8\uba74\uacfc \uc595\uc740 \uacbd\ud654 \uae4a\uc774\uc5d0 \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ub2e4\uc774\uc544\ubaac\ub4dc \uc555\uc785\uc790, \ub85c\ud06c\uc6f0 15N, 30N \ubc0f 45N \uc2a4\ucf00\uc77c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uce21\uc815\uac12<\/th><th class=\"has-text-align-left\" data-align=\"left\">3.175<br>0.125 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">6.350<br>0.250 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">9.525<br>0.375 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">12.700<br>0.500 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">15.875<br>0.625 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">19.050<br>0.750 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">22.225<br>0.875 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">25.400<br>1.000 in.<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">85<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">1.588 mm(1\/16 in.) \ubcfc \uc555\uc785\uc790, \ub85c\ud06c\uc6f0 15T, 30T \ubc0f 45T \uc2a4\ucf00\uc77c<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uce21\uc815\uac12<\/th><th class=\"has-text-align-left\" data-align=\"left\">3.175<br>0.125 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">6.350<br>0.250 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">9.525<br>0.375 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">12.700<br>0.500 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">15.875<br>0.625 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">19.050<br>0.750 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">22.225<br>0.875 in.<\/th><th class=\"has-text-align-left\" data-align=\"left\">25.400<br>1.000 in.<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98: ASM Handbook, Vol. 8, \ud45c\uba74 \ub85c\ud06c\uc6f0 \uacbd\ub3c4 \uc2dc\ud5d8\uae30\ub85c \uc2dc\ud5d8\ud55c \uc6d0\ud1b5\ud615 \uacf5\uc791\ubb3c\uc758 \ubcf4\uc815 \uacc4\uc218. \uc6d0\ubcf8 \ud45c\uc5d0\uc11c 15T, 30T \ubc0f 45T \uc2a4\ucf00\uc77c\uc758 22.225 mm \uc5f4\uc740 \ube44\uc5b4 \uc788\uc2b5\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc2e4\ubb34\uc5d0\uc11c \ubcf4\uc815\uc774 \uac16\ub294 \uc758\ubbf8<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">6.35 mm \ubd09\uc7ac\uc5d0\uc11c 60 HRC \uce21\uc815\uac12\uc740 1.5 \ud3ec\uc778\ud2b8\uc758 \ubcf4\uc815\uc774 \ud544\uc694\ud558\uace0 30 HRC \uce21\uc815\uac12\uc740 5.0 \ud3ec\uc778\ud2b8\uac00 \ud544\uc694\ud569\ub2c8\ub2e4. \uacf5\uad6c\uac15\uc774 \uc0ac\uc6a9\ub418\ub294 \uacbd\ub3c4\uc5d0\uc11c\ub294 \ubcf4\uc815\uc774 \uc791\uc9c0\ub9cc \uc2dc\ud5d8\uc758 \ubc18\ubcf5\uc131\ubcf4\ub2e4 \ud06c\ubbc0\ub85c, \ubd09\uc7ac\uac00 \uc881\uc740 \ud5c8\uc6a9 \ubc94\uc704 \ub0b4\uc5d0 \uc788\ub294\uc9c0\ub97c \uacb0\uc815\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc9c1\uacbd\uc744 \uba85\uc2dc\ud558\uc9c0 \uc54a\uace0 \ud658\ubd09\uc5d0\uc11c 58.5 HRC\ub97c \uc81c\uc2dc\ud55c \uc131\uc801\uc11c\ub294 \ud3c9\uba74 \uc2dc\ud5d8\ud3b8 \uacb0\uacfc\uc640 \ube44\uad50\ud560 \uc218 \uc5c6\uc2b5\ub2c8\ub2e4. \uc9c1\uacbd, \uc2a4\ucf00\uc77c \ubc0f \ud558\uc911\uc744 \uba85\uc2dc\ud558\uace0 \ubcf4\uc815 \uc801\uc6a9 \uc5ec\ubd80\ub97c \ubc1d\ud788\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub3d9\uc77c\ud55c \ud45c\ub294 \ub0b4\uacbd\uc774 \uc624\ubaa9\ud55c \ud45c\uba74\uc778 \uad00\uc7ac\uc640, \uce21\uc815\uac12\uc774 \uc77c\ubc18 \uc2a4\ucf00\uc77c \ubc94\uc704 \uc544\ub798\ub85c \ub5a8\uc5b4\uc9c0\ub294 \uc120\uc7ac\uc5d0\ub3c4 \uc801\uc6a9\ub429\ub2c8\ub2e4. \uc9c1\uacbd 6.35 mm \uc774\ud558\uc5d0\uc11c\ub294 \uc77c\ubc18 \uc2a4\ucf00\uc77c\uc744 \uc0ac\uc6a9\ud560 \uc218 \uc5c6\uc73c\uba70, \ud45c\uba74 N \uc2a4\ucf00\uc77c\uc774 3.175 mm\uae4c\uc9c0 \ubcf4\uc815\uc744 \uc801\uc6a9\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uacbd\ub3c4 \uac12\uc744 \uc81c\uc2dc\ud558\uae30 \uc804\uc5d0<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uacbd\ub3c4 \uce21\uc815\uac12\uc740 \uc2a4\ucf00\uc77c, \ud558\uc911 \ubc0f \ubd80\ud488 \ud615\uc0c1\uc5d0 \uc18d\ud569\ub2c8\ub2e4. \uace1\uba74\uc5d0\uc11c \uce21\uc815\ud55c \uac12\uc744 \ud3c9\uba74 \uc2dc\ud5d8\ud3b8\uacfc \ube44\uad50\ud558\uac70\ub098 \ud45c\uba74 \ub85c\ud06c\uc6f0 \uac12\uc744 C \uc2a4\ucf00\uc77c \uac12\uacfc \ube44\uad50\ud558\uba74 \uc7ac\uc9c8\uacfc \ubb34\uad00\ud55c \ubd88\uc77c\uce58\uac00 \ubc1c\uc0dd\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \ud398\uc774\uc9c0\uc758 \uacc4\uc218\ub294 \uacf5\uac1c\ub41c \ucc38\uc870 \ub370\uc774\ud130\uc774\uba70 \uad6c\uc870\uc801\uc73c\ub85c \uadfc\uc0ac\uac12\uc785\ub2c8\ub2e4. \uc790\uc0ac \uc81c\ud488\uc5d0 \uc801\uc6a9\ub418\ub294 \ud45c\uc900\uc5d0 \ub530\ub77c \ud5c8\uc6a9 \uae30\uc900\uc744 \ud655\uc778\ud558\uace0, \uc131\uc801\uc11c\uc5d0 \uc2a4\ucf00\uc77c, \ud558\uc911, \uc704\uce58 \ubc0f \ubd80\ud488 \uc9c1\uacbd\uc744 \uba85\uc2dc\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \uc0ac\uc774\ud2b8\uc758 \uad00\ub828 \ucc38\uc870 \ud398\uc774\uc9c0: <a href=\"https:\/\/aobosteel.com\/ko\/minimum-thickness-for-hardness-testing\/\">\uacbd\ub3c4 \uc2dc\ud5d8\uc744 \uc704\ud55c \ucd5c\uc18c \ub450\uaed8<\/a>, <a href=\"https:\/\/aobosteel.com\/ko\/hardness-testing-methods\/\">\uacbd\ub3c4 \uc2dc\ud5d8 \ubc29\ubc95<\/a>, <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-hardness-conversion-calculator\/\">\uacf5\uad6c\uac15 \uacbd\ub3c4 \ud658\uc0b0 \uacc4\uc0b0\uae30<\/a>, <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-quality-verification\/\">\uacf5\uad6c\uac15 \ud488\uc9c8 \uac80\uc99d<\/a>, <a href=\"https:\/\/aobosteel.com\/ko\/tool-steels\/\">\uacf5\uad6c\uac15 \uacf5\uae09<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98: ASM Handbook, Volume 8, Mechanical Testing and Evaluation (ASM International), Andrew Fee, Consultant\uc758 \ub17c\ubb38 Selection and Industrial Applications of Hardness Tests \ubc0f Edward L. Tobolski, Wilson Instruments Division, Instron Corporation and Andrew Fee, Consultant\uc758 \ub17c\ubb38 Macroindentation Hardness Testing. \uac12\uc740 \ucc38\uc870\uc6a9\uc73c\ub85c\ub9cc \uc7ac\ud604\ub418\uc5c8\uc2b5\ub2c8\ub2e4. Aobo Steel\uc740 \ud480\ub9bc \uc0c1\ud0dc\uc758 \uacf5\uad6c\uac15\uc744 \uacf5\uae09\ud569\ub2c8\ub2e4.<\/em><\/p>","protected":false},"excerpt":{"rendered":"<p>Hardness Test Correction Factors for Round Bar A hardness reading taken on a round bar is not the same value as a reading taken on flat stock of the same material. This page carries the published correction factors for cylindrical workpieces on the Rockwell scales, with the diameter limits that decide when a correction is [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-19287","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.7 (Yoast SEO v28.7) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Rockwell Hardness Correction for Round Bar | Aobo Steel<\/title>\n<meta name=\"description\" content=\"Correction factors that convert Rockwell hardness readings taken on round bar and tube into flat surface values, on the HRC, HRA, B and superficial N and T scales.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/hardness-test-correction-factors-round-bar\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Hardness Test Correction Factors for Round Bar\" \/>\n<meta property=\"og:description\" content=\"Correction factors that convert Rockwell hardness readings taken on round bar and tube into flat surface values, on the HRC, HRA, B and superficial N and T scales.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/hardness-test-correction-factors-round-bar\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-22T04:10:48+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"4\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hardness-test-correction-factors-round-bar\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hardness-test-correction-factors-round-bar\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Hardness Test Correction Factors for Round Bar\",\"datePublished\":\"2026-09-18T23:33:13+00:00\",\"dateModified\":\"2026-10-22T04:10:48+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hardness-test-correction-factors-round-bar\\\/\"},\"wordCount\":874,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hardness-test-correction-factors-round-bar\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/hardness-test-correction-factors-round-bar\\\/\",\"name\":\"Rockwell Hardness Correction for Round Bar | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-18T23:33:13+00:00\",\"dateModified\":\"2026-10-22T04:10:48+00:00\",\"description\":\"Correction factors that convert Rockwell hardness readings taken on round bar and tube into flat surface values, on the HRC, HRA, B and superficial N and T scales.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hardness-test-correction-factors-round-bar\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/hardness-test-correction-factors-round-bar\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/hardness-test-correction-factors-round-bar\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Hardness Test Correction Factors for Round Bar\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Rockwell Hardness Correction for Round Bar | Aobo Steel","description":"Correction factors that convert Rockwell hardness readings taken on round bar and tube into flat surface values, on the HRC, HRA, B and superficial N and T scales.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/hardness-test-correction-factors-round-bar\/","og_locale":"ko_KR","og_type":"article","og_title":"Hardness Test Correction Factors for Round Bar","og_description":"Correction factors that convert Rockwell hardness readings taken on round bar and tube into flat surface values, on the HRC, HRA, B and superficial N and T scales.","og_url":"https:\/\/aobosteel.com\/ko\/hardness-test-correction-factors-round-bar\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-22T04:10:48+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"4\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/hardness-test-correction-factors-round-bar\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/hardness-test-correction-factors-round-bar\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Hardness Test Correction Factors for Round Bar","datePublished":"2026-09-18T23:33:13+00:00","dateModified":"2026-10-22T04:10:48+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/hardness-test-correction-factors-round-bar\/"},"wordCount":874,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/hardness-test-correction-factors-round-bar\/","url":"https:\/\/aobosteel.com\/hardness-test-correction-factors-round-bar\/","name":"Rockwell Hardness Correction for Round Bar | Aobo Steel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-18T23:33:13+00:00","dateModified":"2026-10-22T04:10:48+00:00","description":"Correction factors that convert Rockwell hardness readings taken on round bar and tube into flat surface values, on the HRC, HRA, B and superficial N and T scales.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/hardness-test-correction-factors-round-bar\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/hardness-test-correction-factors-round-bar\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/hardness-test-correction-factors-round-bar\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Hardness Test Correction Factors for Round Bar"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Hardness Test Correction Factors for Round Bar A hardness reading taken on a round bar is not the same value as a reading taken on flat stock of the same material. This page carries the published correction factors for cylindrical workpieces on the Rockwell scales, with the diameter limits that decide when a correction is&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Hardness Test Correction Factors for Round Bar A hardness reading taken on a round bar is not the same value as a reading taken on flat stock of the same material. This page carries the published correction factors for cylindrical workpieces on the Rockwell scales, with the diameter limits that decide when a correction is&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19287","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=19287"}],"version-history":[{"count":5,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19287\/revisions"}],"predecessor-version":[{"id":24083,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/19287\/revisions\/24083"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=19287"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}