{"id":18292,"date":"2026-09-14T18:58:31","date_gmt":"2026-09-14T10:58:31","guid":{"rendered":"https:\/\/aobosteel.com\/tool-steel-tempering-chart\/"},"modified":"2026-10-18T23:06:51","modified_gmt":"2026-10-18T15:06:51","slug":"tool-steel-tempering-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/tool-steel-tempering-chart\/","title":{"rendered":"\ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uac00\uacf5 \uacbd\ub3c4"},"content":{"rendered":"<h1 class=\"wp-block-heading has-text-align-center\" id=\"h-tool-steel-tempering-chart\">\uacf5\uad6c\uac15 \ud15c\ud37c\ub9c1 \ucc28\ud2b8<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\ud15c\ud37c\ub9c1 \uc628\ub3c4, \uac01 \uc628\ub3c4\uc5d0\uc11c \uc5bb\uc5b4\uc9c0\ub294 \uacbd\ub3c4, \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/temper-color-time-chart\/\">\ud604\uc7a5\uc5d0\uc11c \uc628\ub3c4\ub97c \ud310\ub2e8\ud558\ub294 \ub370 \uc0ac\uc6a9\ub418\ub294 \uc0b0\ud654 \uc0c9\uc0c1<\/a>. D2, D3, D4, D5, D7, O1, O2, O6, O7, A2, A6, A7, A8, H10~H23, <a href=\"https:\/\/aobosteel.com\/ko\/m2-steel-specifications\/\">M2<\/a>, M4 \ubc0f M42\ub97c \ub2e4\ub8e8\uba70, \ubbf8\ud130\ubc95 \ubc0f \uc57c\ub4dc\ud30c\uc6b4\ub4dc\ubc95 \uac12\uc744 \ud3ec\ud568\ud569\ub2c8\ub2e4.<\/p>\n\n\n<h2 class=\"wp-block-post-title\">\ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uac00\uacf5 \uacbd\ub3c4<\/h2>\n\n\n<p class=\"wp-block-paragraph\">6\uac1c \ub4f1\uae09\uc774 \ub300\ubd80\ubd84\uc758 \uae08\ud615 \ubc0f \uacf5\uad6c \uc791\uc5c5\uc744 \ucee4\ubc84\ud558\uba70, \uac01 \ub4f1\uae09\uc774 \ud1b5\uc0c1 \uc0ac\uc6a9\ub418\ub294 \uacbd\ub3c4\ub97c \uc81c\uc2dc\ud569\ub2c8\ub2e4. \ub2f4\uae08\uc9c8 \uc628\ub3c4\uc640 \uc804\uccb4 \ub2f4\uae08\uc9c8-\ud15c\ud37c\ub9c1 \uc77c\uc815\uc740 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-hardening-tempering-chart\/\">\uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1 \ucc28\ud2b8<\/a>.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc720\ud615<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uae09\ub7ad\ub41c HRC <sup>(a)<\/sup><\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC\uc5d0\uc11c \uadfc\ubb34<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uad8c\uc7a5 \ud15c\ud37c\ub9c1 \uc628\ub3c4, \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0C<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel\/\">A2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0c9\uac04 \uac00\uacf5, \uacf5\uae30 \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><td class=\"has-text-align-left\" data-align=\"left\">58\u201360<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u2013450<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013232<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel\/\">D2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0c9\uac04 \uac00\uacf5, \uace0\ud06c\ub86c<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><td class=\"has-text-align-left\" data-align=\"left\">58\u201360<\/td><td class=\"has-text-align-left\" data-align=\"left\">900\u2013960<\/td><td class=\"has-text-align-left\" data-align=\"left\">482\u2013516<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel\/\">H13<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\uc628 \uc791\uc5c5, \ud06c\ub86c<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><td class=\"has-text-align-left\" data-align=\"left\">40\u201348<\/td><td class=\"has-text-align-left\" data-align=\"left\">1050\u20131150<\/td><td class=\"has-text-align-left\" data-align=\"left\">566\u2013621<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/m2-tool-steel\/\">M2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\uc18d\ub3c4 \ubab0\ub9ac\ube0c\ub374<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">62\u201364<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131050<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013566<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/o1-tool-steel\/\">O1<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0c9\uac04 \uac00\uacf5, \uc624\uc77c \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><td class=\"has-text-align-left\" data-align=\"left\">58\u201360<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u2013450<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013232<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/s7-tool-steel\/\">S7<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9 \ubc29\uc9c0<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">56\u201358<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u2013450<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013232<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: \uacf5\uad6c \ubc0f \uae08\ud615 \uc81c\uc791 \ubb38\uc81c \ud574\uacb0\uc0ac(RM Leed), \ud45c 8-7, \ubca0\ub4e4\ub808\ud5f4 \uc2a4\ud2f8 \uc790\ub8cc.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uacf5\uad6c\uac15 \ud15c\ud37c\ub9c1 \ucc28\ud2b8, \uc778\uc1c4\uc6a9 PDF<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">28\uac1c \ub4f1\uae09\uc758 \ud15c\ud37c\ub9c1 \ubc94\uc704, H13 \ubc0f M2 \uacbd\ub3c4 \ub370\uc774\ud130, \uc0b0\ud654 \ud15c\ud37c\ub9c1 \uc0c9\uc0c1, \uadf8\ub9ac\uace0 \ub2f9\uc0ac \uc5f0\ub77d\ucc98\ub97c \ub2f4\uc740 A4 \uc138 \ud398\uc774\uc9c0 \ubd84\ub7c9.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Tempering-Chart.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 510 KB<\/a><\/div>\n<\/div>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">\ub4f1\uae09\ubcc4 \ud15c\ud37c\ub9c1 \ubc94\uc704<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uac00\uc7a5 \ub9ce\uc774 \uc778\uc6a9\ub418\uace0 \uc7ac\uace0\ub85c \ubcf4\uc720\ub41c \uacf5\uad6c\uac15\uc758 \uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1 \ub370\uc774\ud130\uc785\ub2c8\ub2e4. \uacc4\uc5f4\ubcc4\ub85c \ubd84\ub958\ud588\uc73c\uba70 \ud15c\ud37c\ub9c1 \ubc94\uc704\uc5d0 \uac78\uce5c \ub300\ub7b5\uc801\uc778 \uacbd\ub3c4 \ud3ed\uc744 \ud568\uaed8 \uc815\ub9ac\ud588\uc2b5\ub2c8\ub2e4. \uac01 \ub4f1\uae09\uc758 \ud654\ud559 \uc870\uc131\uc740 \ub2e4\uc74c\uc744 \ucc38\uc870\ud558\uc2ed\uc2dc\uc624: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-composition-chart\/\">\uacf5\uad6c\uac15 \uc870\uc131 \ucc28\ud2b8<\/a>.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc720\ud615<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4, \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub300\ub7b5\uc801\uc778 \ub2f4\uae08\uc9c8 \uacbd\ub3c4, HRC <sup>(c)<\/sup><\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\"><a href=\"https:\/\/aobosteel.com\/ko\/high-speed-steels\/\">\uace0\uc18d \uacf5\uad6c\uac15<\/a><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/m2-tool-steel-heat-treatment\/\">M2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubab0\ub9ac\ube0c\ub374\uacc4 \uace0\uc18d\ub3c4\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131160<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013627<\/td><td class=\"has-text-align-left\" data-align=\"left\">65\u201360<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/m4-tool-steel-heat-treatment\/\">M4<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubab0\ub9ac\ube0c\ub374\uacc4 \uace0\uc18d\ub3c4\uac15, \ubc14\ub098\ub4d0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131100<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013593<\/td><td class=\"has-text-align-left\" data-align=\"left\">66\u201361<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/m7-tool-steel-heat-treatment\/\">M7<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubab0\ub9ac\ube0c\ub374\uacc4 \uace0\uc18d\ub3c4\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131100<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013593<\/td><td class=\"has-text-align-left\" data-align=\"left\">66\u201361<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubab0\ub9ac\ube0c\ub374\uacc4 \uace0\uc18d\ub3c4\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131100<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013593<\/td><td class=\"has-text-align-left\" data-align=\"left\">65\u201360<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/m42-tool-steel\/\">M42<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucf54\ubc1c\ud2b8\uacc4 \uace0\uc18d\ub3c4\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">950\u20131100<\/td><td class=\"has-text-align-left\" data-align=\"left\">510\u2013593<\/td><td class=\"has-text-align-left\" data-align=\"left\">70\u201365<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\"><a href=\"https:\/\/aobosteel.com\/ko\/hot-work-tool-steels\/\">\uace0\uc628 \uc791\uc5c5\uc6a9 \uacf5\uad6c\uac15<\/a><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/h10-tool-steel-heat-treatment-guide\/\">H10<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c\uacc4 \uc5f4\uac04\uacf5\uad6c\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131200<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013649<\/td><td class=\"has-text-align-left\" data-align=\"left\">56\u201339<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/h11-tool-steel-heat-treatment\/\">H11<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c\uacc4 \uc5f4\uac04\uacf5\uad6c\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131200<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013649<\/td><td class=\"has-text-align-left\" data-align=\"left\">54\u201338<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/h12-tool-steel-heat-treatment\/\">H12<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c-\ud145\uc2a4\ud150 \uc5f4\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131200<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013649<\/td><td class=\"has-text-align-left\" data-align=\"left\">55\u201338<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/h13-steel-heat-treatment\/\">H13<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c\uacc4 \uc5f4\uac04\uacf5\uad6c\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131200<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013649<\/td><td class=\"has-text-align-left\" data-align=\"left\">53\u201338<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/h19-tool-steel-heat-treatment\/\">H19<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c-\ucf54\ubc1c\ud2b8 \uc5f4\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000\u20131300<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013704<\/td><td class=\"has-text-align-left\" data-align=\"left\">59\u201340<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/h21-tool-steel\/\">H21<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud145\uc2a4\ud150\uacc4 \uc5f4\uac04\uacf5\uad6c\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1100\u20131250<\/td><td class=\"has-text-align-left\" data-align=\"left\">593\u2013677<\/td><td class=\"has-text-align-left\" data-align=\"left\">54\u201336<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H23<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud145\uc2a4\ud150\uacc4 \uc5f4\uac04\uacf5\uad6c\uac15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200\u20131500<\/td><td class=\"has-text-align-left\" data-align=\"left\">649\u2013816<\/td><td class=\"has-text-align-left\" data-align=\"left\">47\u201330<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\"><a href=\"https:\/\/aobosteel.com\/ko\/cold-work-tool-steels\/\">\ub0c9\uac04 \uac00\uacf5 \uacf5\uad6c\uac15<\/a><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel-heat-treatment-guide\/\">D2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\ud06c\ub86c \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u20131000<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013538<\/td><td class=\"has-text-align-left\" data-align=\"left\">61\u201354<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/d3-tool-steel-heat-treatment\/\">D3<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\ud06c\ub86c \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u20131000<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013538<\/td><td class=\"has-text-align-left\" data-align=\"left\">61\u201354<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\ud06c\ub86c \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u20131000<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013538<\/td><td class=\"has-text-align-left\" data-align=\"left\">61\u201354<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\ud06c\ub86c \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u20131000<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013538<\/td><td class=\"has-text-align-left\" data-align=\"left\">61\u201354<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\ud06c\ub86c \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">300\u20131000<\/td><td class=\"has-text-align-left\" data-align=\"left\">149\u2013538<\/td><td class=\"has-text-align-left\" data-align=\"left\">65\u201358<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel-heat-treatment-guide\/\">A2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\ud569\uae08 \uacf5\uae30 \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">350\u20131000<\/td><td class=\"has-text-align-left\" data-align=\"left\">177\u2013538<\/td><td class=\"has-text-align-left\" data-align=\"left\">62\u201357<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\ud569\uae08 \uacf5\uae30 \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">300\u2013800<\/td><td class=\"has-text-align-left\" data-align=\"left\">149\u2013427<\/td><td class=\"has-text-align-left\" data-align=\"left\">60\u201354<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\ud569\uae08 \uacf5\uae30 \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">300\u20131000<\/td><td class=\"has-text-align-left\" data-align=\"left\">149\u2013538<\/td><td class=\"has-text-align-left\" data-align=\"left\">67\u201357<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\ud569\uae08 \uacf5\uae30 \uacbd\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">350\u20131100<\/td><td class=\"has-text-align-left\" data-align=\"left\">177\u2013593<\/td><td class=\"has-text-align-left\" data-align=\"left\">60\u201350<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/o1-tool-steel-heat-treatment\/\">O1<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">350\u2013500<\/td><td class=\"has-text-align-left\" data-align=\"left\">177\u2013260<\/td><td class=\"has-text-align-left\" data-align=\"left\">62\u201357<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/o2-tool-steel-heat-treatment\/\">O2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">350\u2013500<\/td><td class=\"has-text-align-left\" data-align=\"left\">177\u2013260<\/td><td class=\"has-text-align-left\" data-align=\"left\">62\u201357<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/o6-tool-steel-heat-treatment\/\">O6<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">350\u2013600<\/td><td class=\"has-text-align-left\" data-align=\"left\">177\u2013316<\/td><td class=\"has-text-align-left\" data-align=\"left\">63\u201358<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">350\u2013550<\/td><td class=\"has-text-align-left\" data-align=\"left\">177\u2013288<\/td><td class=\"has-text-align-left\" data-align=\"left\">64\u201358<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\"><a href=\"https:\/\/aobosteel.com\/ko\/s-series-tool-steel\/\">\ub0b4\ucda9\uaca9\uc131 \uacf5\uad6c\uac15<\/a><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/s1-tool-steel-heat-treatment-guide\/\">S1<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9 \ubc29\uc9c0<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u20131200<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013649<\/td><td class=\"has-text-align-left\" data-align=\"left\">58\u201340<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/s5-tool-steel-heat-treatment\/\">S5<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9 \ubc29\uc9c0<\/td><td class=\"has-text-align-left\" data-align=\"left\">350\u2013800<\/td><td class=\"has-text-align-left\" data-align=\"left\">177\u2013427<\/td><td class=\"has-text-align-left\" data-align=\"left\">60\u201350<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/s7-tool-steel-heat-treatment\/\">S7<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucda9\uaca9 \ubc29\uc9c0<\/td><td class=\"has-text-align-left\" data-align=\"left\">400\u20131150<\/td><td class=\"has-text-align-left\" data-align=\"left\">204\u2013621<\/td><td class=\"has-text-align-left\" data-align=\"left\">57\u201345<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: Machinery\u2019s Handbook, 28th ed., \uacf5\uad6c\uac15 \ud45c 6, 8, 9, 10(\uace0\uc18d\ub3c4\uac15, \uc5f4\uac04\uac00\uacf5\uac15, \ub0c9\uac04\uac00\uacf5\uac15, \ub0b4\ucda9\uaca9\uac15 \uadf8\ub8f9).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uac01 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uc5d0\uc11c\uc758 H13<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774\uc911 \ud15c\ud37c\ub9c1 \ud6c4 H13\uc758 \uacbd\ub3c4, \uc778\uc7a5 \ud2b9\uc131 \ubc0f \ucda9\uaca9 \uc5d0\ub108\uc9c0. \ub3d9\uc77c\ud55c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4, \ub450 \uac00\uc9c0 \ub2f4\uae08\uc9c8 \uacbd\ub85c. \uc791\uc5c5 \uc628\ub3c4\uc5d0\uc11c\uc758 \uacbd\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-hot-hardness-chart\/\">\uace0\uc628 \uacbd\ub3c4\ud45c<\/a>.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub728\uc784 <br>\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4<br>HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5\ub825<br>MPa(ksi)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc0dd\uc0b0\ud558\ub2e4<br>MPa(ksi)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc7a5<br>%<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc0e4\ub974\ud53c V-\ub178\uce58<br>at 21 \u00b0C, J (ft\u00b7lbf)<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"7\">1010 \u00b0C(1850 \u00b0F)\uc5d0\uc11c \uc720\ub2f4\uae08\uc9c8, 2 + 2\uc2dc\uac04 \uc774\uc911 \ud15c\ud37c\ub9c1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">527<\/td><td class=\"has-text-align-left\" data-align=\"left\">980<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">1960 (284)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1570 (228)<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">16 (12)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">555<\/td><td class=\"has-text-align-left\" data-align=\"left\">1030<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">1835 (266)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1530 (222)<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">24 (18)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">575<\/td><td class=\"has-text-align-left\" data-align=\"left\">1065<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">1730 (251)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1470 (213)<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 (20)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">593<\/td><td class=\"has-text-align-left\" data-align=\"left\">1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">46<\/td><td class=\"has-text-align-left\" data-align=\"left\">1580 (229)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1365 (198)<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.5 (21)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"7\">1010 \u00b0C(1850 \u00b0F)\uc5d0\uc11c \uacf5\ub7ad, 2 + 2\uc2dc\uac04 \uc774\uc911 \ud15c\ud37c\ub9c1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">524<\/td><td class=\"has-text-align-left\" data-align=\"left\">975<\/td><td class=\"has-text-align-left\" data-align=\"left\">54<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">14 (10)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">565<\/td><td class=\"has-text-align-left\" data-align=\"left\">1050<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">14 (10)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">607<\/td><td class=\"has-text-align-left\" data-align=\"left\">1125<\/td><td class=\"has-text-align-left\" data-align=\"left\">47<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">24 (18)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Volume 1(10th ed.), Ultrahigh-Strength Steels, \ud45c 31 \ubc0f 33(H13 \ud658\ubd09). \uacf5\ub7ad \uc2dc\ub9ac\uc988\ub294 \uacbd\ub3c4\uc640 \ucda9\uaca9 \uc5d0\ub108\uc9c0\ub9cc \ubcf4\uace0\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \uacbd\ub3c4\uc640 \ud15c\ud37c\ub9c1 \uc628\ub3c4 \uac04\uc758 \uad00\uacc4<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">700~1050 \u00b0F \uc0ac\uc774\uc758 \ud558\ub77d\uacfc \ud68c\ubcf5\uc740 2\ucc28 \uacbd\ud654\uc774\uba70, \uc774\uac83\uc774 \uace0\uc18d\ub3c4\uac15\uc744 \ub2e8\uc21c\ud788 \uacbd\ud654\uc2dc\ud0a4\ub294 \ub300\uc2e0 \uace0\uc628\uc5d0\uc11c \ud15c\ud37c\ub9c1\ud558\ub294 \uc774\uc720\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub728\uc784<br>\u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \ub2f4\uae08\uc9c8 \ud6c4 \uacbd\ub3c4, HRC<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacf5\ub7ad \ud6c4 \uacbd\ub3c4, HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">66<\/td><td class=\"has-text-align-left\" data-align=\"left\">66.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">400<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">500<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">63<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">700<\/td><td class=\"has-text-align-left\" data-align=\"left\">370<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">800<\/td><td class=\"has-text-align-left\" data-align=\"left\">425<\/td><td class=\"has-text-align-left\" data-align=\"left\">63<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">900<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">540<\/td><td class=\"has-text-align-left\" data-align=\"left\">66<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1050<\/td><td class=\"has-text-align-left\" data-align=\"left\">565<\/td><td class=\"has-text-align-left\" data-align=\"left\">66<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">595<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1150<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">62<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">53<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: Heat Treatment, Selection and Application of Tool Steels(W. E. Bryson, 2nd ed.), \ud45c 10.1, 2250 \u00b0F(1230 \u00b0C)\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc0c9\uc0c1 \uc870\uc808<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc77c\ubc18 \ud0c4\uc18c\uac15\uc5d0 \ub098\ud0c0\ub098\ub294 \uc0b0\ud654\ub9c9 \uc0c9\uc0c1\uc740 \uace0\uc628\uacc4\uac00 \uc5c6\uc744 \ub54c \uc791\uc5c5 \ud604\uc7a5\uc5d0\uc11c \uc628\ub3c4\ub97c \ud655\uc778\ud558\ub294 \ub370 \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uac15\ucca0\uc758 \uc0c9\uc0c1<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">430<\/td><td class=\"has-text-align-left\" data-align=\"left\">221<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc544\uc8fc \uc5f0\ud55c \ub178\ub780\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">440<\/td><td class=\"has-text-align-left\" data-align=\"left\">227<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\ud55c \ub178\ub780\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><td class=\"has-text-align-left\" data-align=\"left\">232<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc605\uc740 \uc9da\uc0c9 \ub178\ub780\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">460<\/td><td class=\"has-text-align-left\" data-align=\"left\">238<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9da\uc0c9 \ub178\ub780\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">470<\/td><td class=\"has-text-align-left\" data-align=\"left\">243<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c4\ud55c \uc9da\uc0c9 \ub178\ub780\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">249<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c4\ud55c \ub178\ub780\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">490<\/td><td class=\"has-text-align-left\" data-align=\"left\">254<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud669\uac08\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">500<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uac08\uc0c9-\ub178\ub780\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">510<\/td><td class=\"has-text-align-left\" data-align=\"left\">266<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubd89\uc740 \uac08\uc0c9 \ubc18\uc810<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">520<\/td><td class=\"has-text-align-left\" data-align=\"left\">271<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uac08\uc0c9-\ubcf4\ub77c\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">530<\/td><td class=\"has-text-align-left\" data-align=\"left\">277<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\ubcf4\ub77c\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">540<\/td><td class=\"has-text-align-left\" data-align=\"left\">282<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc644\uc804\ud55c \ubcf4\ub77c\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">288<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c4\ud55c \ubcf4\ub77c\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">560<\/td><td class=\"has-text-align-left\" data-align=\"left\">293<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc644\uc804 \ud30c\ub780\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">570<\/td><td class=\"has-text-align-left\" data-align=\"left\">299<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c4\uccad\uc0c9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">640<\/td><td class=\"has-text-align-left\" data-align=\"left\">338<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\ud55c \ud30c\ub780\uc0c9<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: Machinery\u2019s Handbook, 28th ed., \ud45c 1, \ud0c4\uc18c\uac15\uc758 \uc0c9\uc0c1\uc73c\ub85c \ud45c\uc2dc\ub418\ub294 \uc628\ub3c4. \ub2e4\ub978 \ud604\uc7a5 \uc790\ub8cc\uc5d0\uc11c\ub294 \ub3d9\uc77c\ud55c \uc0c9\uc0c1\uc744 \uc57d\uac04 \ub2e4\ub978 \ubc94\uc704\ub85c \uc81c\uc2dc\ud569\ub2c8\ub2e4. \uc608\ub97c \ub4e4\uc5b4 \ubc00\uc9da\uc0c9\uc740 460 \u00b0F(238 \u00b0C), \uccad\uc0c9\uc740 580 \u00b0F(304 \u00b0C)\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uacf5\uad6c\uac15 \ud15c\ud37c\ub9c1 \ucc28\ud2b8, \uc778\uc1c4\uc6a9 PDF<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">28\uac1c \ub4f1\uae09\uc758 \ud15c\ud37c\ub9c1 \ubc94\uc704, H13 \ubc0f M2 \uacbd\ub3c4 \ub370\uc774\ud130, \uc0b0\ud654 \ud15c\ud37c\ub9c1 \uc0c9\uc0c1, \uadf8\ub9ac\uace0 \ub2f9\uc0ac \uc5f0\ub77d\ucc98\ub97c \ub2f4\uc740 A4 \uc138 \ud398\uc774\uc9c0 \ubd84\ub7c9.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Tempering-Chart.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 510 KB<\/a><\/div>\n<\/div>\n<\/div>\n\n\n\n<ul class=\"wp-block-list\">\n<li><sup>(a)<\/sup> \ub2f4\uae08\uc9c8 \uc9c1\ud6c4\uc758 \uacbd\ub3c4\ub294 \ud15c\ud37c\ub9c1 \uc804\uc5d0 \uce21\uc815\ud55c \uac12\uc785\ub2c8\ub2e4.<\/li>\n\n\n\n<li><sup>(b)<\/sup> \uc628\ub3c4\ub294 \uac01 \ucd9c\ucc98\uc5d0 \uac8c\uc2dc\ub41c \uadf8\ub300\ub85c \ud45c\uae30\ud588\uc2b5\ub2c8\ub2e4. \ud15c\ud37c\ub9c1 \uacbd\ub3c4\ud45c\uc758 \uc12d\uc528 \uac12\uc740 \ud654\uc528 \uac12\uc744 \uc12d\uc528\ub85c \ubcc0\ud658\ud55c \ud6c4 \uac00\uc7a5 \uac00\uae4c\uc6b4 \uc815\uc218\ub85c \ubc18\uc62c\ub9bc\ud588\uc2b5\ub2c8\ub2e4.<\/li>\n\n\n\n<li><sup>(c)<\/sup> \ub300\ub7b5\uc801\uc778 \ud15c\ud37c\ub9c1 \uacbd\ub3c4\ub294 \ub2e4\uc74c\uc758 \ud558\ud55c\uc5d0\uc11c <a href=\"https:\/\/aobosteel.com\/ko\/carbon-tool-steel-temper-chart\/\">\ud15c\ud37c\ub9c1 \uc708\ub3c4\uc6b0<\/a> \uc0c1\ud55c\uae4c\uc9c0\uc785\ub2c8\ub2e4. \uc815\ud655\ud55c \uac12\uc740 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4, \ub2f4\uae08\uc9c8, \ub2e8\uba74 \ud06c\uae30 \ubc0f \ud15c\ud37c\ub9c1 \ud69f\uc218\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9d1\ub2c8\ub2e4.<\/li>\n<\/ul>\n\n\n\n<h3 id=\"h-table-notes\" class=\"wp-block-heading\">\ud14c\uc774\ube14 \ub178\ud2b8<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\ub3d9\uc77c\ud55c \ub4f1\uae09\uc5d0 \ub300\ud574 \ucc38\uace0 \ubb38\ud5cc\ub9c8\ub2e4 \ud15c\ud37c\ub9c1 \ubc94\uc704\uac00 \ub2e4\ub974\uac8c \uac8c\uc7ac\ub418\ub294\ub370, \uc774\ub294 \uacb0\uacfc\uac00 \ubd80\ud488\uc758 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ubc29\ubc95, \ub0c9\uac01 \uc18d\ub3c4, \ub450\uaed8 \ubc0f \ud15c\ud37c\ub9c1 \ud69f\uc218\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9c0\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uc608\ub97c \ub4e4\uc5b4 D2\ub294 900~960 \u00b0F(482~516 \u00b0C)\uc5d0\uc11c \ud15c\ud37c\ub9c1\ud558\uc5ec <a href=\"https:\/\/aobosteel.com\/ko\/blog\/best-hrc-for-d2-tool-steel\/\">58~60 HRC<\/a> \ud604\uc7a5 \uad00\ud589\uc5d0\uc11c\ub294 \uc720\uc9c0\ub418\uc9c0\ub9cc, Machinery\u2019s Handbook\uc740 400~1000 \u00b0F\uc758 \ub354 \ub113\uc740 \ubc94\uc704\uc640 \uc57d 61~54 HRC\uc758 \uacbd\ub3c4 \ud3ed\uc744 \uc81c\uc2dc\ud569\ub2c8\ub2e4. \ub450 \ud45c \ubaa8\ub450 \uc2dc\uc791 \ubc94\uc704\ub85c \uac04\uc8fc\ud558\uace0, \uc2dc\ud5d8\ud3b8\uc73c\ub85c \uc790\uccb4 \uc5f4\ucc98\ub9ac\ub85c\uc5d0\uc11c \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li><strong>\ub2f4\uae08\uc9c8 \uc9c1\ud6c4 \ubc14\ub85c \ud15c\ud37c\ub9c1\ud558\uc2ed\uc2dc\uc624.<\/strong> <a href=\"https:\/\/aobosteel.com\/ko\/air-hardening-tool-steel\/\">\uacf5\uae30 \uacbd\ud654<\/a> \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/oil-hardening-tool-steel\/\">\uc720\ub0c9 \uacbd\ud654<\/a> \ub4f1\uae09\uc740 \ubd80\ud488\uc774 \uc544\uc9c1 \ub530\ub73b\ud560 \ub54c(\uc57d 125~150 \u00b0F, 50~65 \u00b0C) \ud15c\ud37c\ub9c1\ub85c\uc5d0 \ub3c4\ub2ec\ud574\uc57c \ud569\ub2c8\ub2e4. \uccab \ud15c\ud37c\ub9c1 \uc804\uc5d0 \uc2e4\uc628\uc5d0 \ubc29\uce58\ub41c \ub2f4\uae08\uc9c8 \uacf5\uad6c\ub294 \ub354 \ub192\uc740 <a href=\"https:\/\/aobosteel.com\/ko\/blog\/how-to-avoid-d2-heat-treatment-mistakes\/\">\uade0\uc5f4 \uc704\ud5d8<\/a>, \uc9c0\uc5f0\uc744 \ud53c\ud558\ub294 \ub370\uc5d0\ub294 \ube44\uc6a9\uc774 \ub4e4\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \ub2e8\uba74 1\uc778\uce58\ub2f9 1\uc2dc\uac04 \ub3d9\uc548 \uc628\ub3c4\ub97c \uc720\uc9c0\ud558\uace0, \ud06c\uac70\ub098 \ubcf5\uc7a1\ud55c \ub2e8\uba74\uc758 \uacbd\uc6b0 1\uc778\uce58\ub2f9 2\uc2dc\uac04 \ub3d9\uc548 \uc720\uc9c0\ud558\uc2ed\uc2dc\uc624. \uacf5\uc815 \ub2e8\uacc4\ub97c \uac74\ub108\ub6f8 \ub54c \ubc1c\uc0dd\ud558\ub294 \uacb0\ud568\uacfc \uc774\ub97c \uc218\uc815\ud558\ub294 \uac80\uc0ac \uc0ac\ud56d\uc740 \ubaa9\ub85d\uc5d0 \ub098\uc640 \uc788\uc2b5\ub2c8\ub2e4. <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-troubleshooting-chart\/\">\uc5f4\ucc98\ub9ac \ubb38\uc81c \ud574\uacb0 \ucc28\ud2b8<\/a>.<\/li>\n<\/ul>\n\n\n\n<ul class=\"wp-block-list\">\n<li><strong>\uace0\uc18d\uac15\uc758 \uacbd\uc6b0 2\ud68c, 3\ud68c \ud15c\ud37c\ub9c1 \ucc98\ub9ac\ub97c \ud569\ub2c8\ub2e4.<\/strong> \uacf5\uae30 \uacbd\ud654 \ub0c9\uac04 \uac00\uacf5 \uac15\uc885\uacfc \ubab0\ub9ac\ube0c\ub374 \uace0\uc18d\ub3c4 \uac15\uc885\uc740 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-tempering-isothermal-transformation\/\">\uc77c\ubc18\uc801\uc73c\ub85c \ub450 \ubc88 \ud15c\ud37c\ub9c1\ud558\uc5ec<\/a> <a href=\"https:\/\/aobosteel.com\/ko\/retained-austenite-tool-steel\/\">\uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8<\/a> \ub97c \uc9c0\ub2c8\uba70 \uce58\uc218\ub97c \uc548\uc815\ud654\ud569\ub2c8\ub2e4. \ud615\uc0c1\uc774 \ubcf5\uc7a1\ud55c \ubd80\ud488\uc774\ub098 \uac00\ud639\ud55c \uc0ac\uc6a9 \uc870\uac74\uc758 \uacf5\uad6c\uc5d0\ub294 3\ucc28 \ud15c\ud37c\ub9c1\uc744 \ucd94\uac00\ud558\uc2ed\uc2dc\uc624.<\/li>\n<\/ul>\n\n\n\n<ul class=\"wp-block-list\">\n<li><strong>\uc5f4\ucc98\ub9ac\ub41c \ubd80\ud488\uc740 \uc808\ub300\ub85c \uc5f4\ucc98\ub9ac \uc628\ub3c4 \uc774\uc0c1\uc73c\ub85c \uac00\uc5f4\ud558\uc9c0 \ub9c8\uc2ed\uc2dc\uc624.<\/strong> \uc751\ub825 \uc81c\uac70, \uad50\uc815 \ub610\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/blog\/d2-tool-steel-weld-repair\/\">\uc6a9\uc811 \uc218\ub9ac<\/a> \uadf8 \uc628\ub3c4 \uc774\uc0c1\uc5d0\uc11c\ub294 \uacf5\uad6c\uac00 \uc5f0\ud574\uc9c0\uae30 \ub54c\ubb38\uc5d0, \ub2f4\uae08\uc9c8 \uc628\ub3c4\ub294 \uc774\ud6c4 \ubaa8\ub4e0 \uacf5\uc815\uc758 \uc0c1\ud55c\uc120\uc744 \uc124\uc815\ud569\ub2c8\ub2e4.<\/li>\n<\/ul>\n\n\n\n<ul class=\"wp-block-list\">\n<li><strong>\uc0c9\uc0c1\uc740 \ub2e8\uc9c0 \ucc38\uace0\uc6a9\uc77c \ubfd0\uc785\ub2c8\ub2e4.<\/strong> \ub9c8\uc9c0\ub9c9 \ud45c\uc758 \uc0b0\ud654\ubb3c \uc0c9\uc0c1\uc740 \ub2e4\uc74c\uc5d0\uc11c \uce21\uc815\ub418\uc5c8\uc2b5\ub2c8\ub2e4. <a href=\"https:\/\/aobosteel.com\/ko\/blog\/1045-vs-tool-steel\/\">\ud0c4\uc18c\uac15<\/a>. \ud569\uae08 \ud568\ub7c9\uc5d0 \ub530\ub77c \uc628\ub3c4\uac00 \ubcc0\ud558\ubbc0\ub85c \uc5f4\uc804\ub300 \ub610\ub294 \uace0\uc628\uacc4\ub97c \uc0ac\uc6a9\ud558\uc5ec \uc628\ub3c4\ub97c \uc81c\uc5b4\ud558\uace0 \uc791\uc5c5 \ud604\uc7a5\uc5d0\uc11c \uc0c9\uc0c1\uc744 \ud1b5\ud574 \uad50\ucc28 \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\">\ud574\ub2f9 \ubd80\ud488\uc740 \uc5ec\uae30\uc5d0 \uc788\uc5b4\uc57c \ud569\ub2c8\ub2e4. <strong>125 to 150 \u00b0F (50 to 65 \u00b0C)<\/strong> \uc5f4\ucc98\ub9ac\ub85c\uc5d0 \ub4e4\uc5b4\uac08 \ub54c \uc644\uc804\ud788 \uc2dd\uc5b4\uc57c \ud569\ub2c8\ub2e4. \uc644\uc804\ud788 \uc2dd\uc744 \ub54c\uae4c\uc9c0 \uae30\ub2e4\ub9ac\uba74 \uacf5\uae30 \uacbd\ud654\ud615 \uac15\uc7ac\uc758 \uacbd\uc6b0 \uade0\uc5f4 \uc704\ud5d8\uc774 \uc99d\uac00\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud574\ub2f9 \uc628\ub3c4\uc5d0\uc11c \ubcf4\uad00\ud558\uc2ed\uc2dc\uc624. <strong>\ub2e8\uba74 1\uc778\uce58\ub2f9 1\uc2dc\uac04<\/strong>, \uc911\ub7c9 \ub610\ub294 \ubcf5\uc7a1\ud55c \ube14\ub85d\uc758 \uacbd\uc6b0 1\uc778\uce58\ub2f9 2\uc2dc\uac04. \uc9e7\uc740 \uc720\uc9c0 \uc2dc\uac04\uc740 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc640 \ubd88\uc548\uc815\ud55c \uce58\uc218\ub97c \ub0a8\uae41\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc791\uc5c5 \ubc94\uc704\ub97c \ucd08\uacfc\ud558\ub294 \ubaa8\ub4e0 \uacbd\ub3c4 \uc9c0\uc810\uc740 \uc778\uc131\uc744 \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4. \uc77c\ubd80 \ub728\uc784 \uc628\ub3c4 \uad6c\uac04\uc740 \ub2e4\ub978 \uc774\uc720\ub85c \uc778\uc131\uc744 \uc800\ud558\uc2dc\ud0a4\uba70, \uac01\uac01\uc744 \uc720\ubc1c\ud558\ub294 \uc628\ub3c4\ub294 \ub2e4\uc74c \ud398\uc774\uc9c0\uc5d0 \ub098\uc5f4\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/steel-embrittlement-types\/\">\uac15 \ucde8\uc131 \uc720\ud615 \ud398\uc774\uc9c0<\/a>. <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-selection-by-application\/\">\ub2e4\uc774\uc5d0 \ud544\uc694\ud55c \ubc94\uc704\ub97c \uc120\ud0dd\ud558\uc138\uc694<\/a> \uadf8\ub9ac\uace0 \uac15\uc7ac\uac00 \uacac\ub51c \uc218 \uc788\ub294 \ucd5c\ub300\uce58\uae4c\uc9c0 \uacbd\ud654\ud558\uae30\ubcf4\ub2e4\ub294 \uadf8 \ubc94\uc704 \uc548\uc5d0\uc11c \uc720\uc9c0\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud15c\ud37c\ub9c1 \ubc94\uc704\ub294 \ub4f1\uae09 \ubc0f \uc81c\uac15\uc0ac\uc5d0 \ub530\ub77c \ub2e4\ub985\ub2c8\ub2e4. Aobo Steel\uc740 \uacf5\uae09\ud569\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-guide\/\">\uc5f4\ucc98\ub9ac \uc9c0\uce68<\/a> \uc8fc\ubb38\ud560 \ub54c\ub9c8\ub2e4, \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/blog\/verify-tool-steel-test-report\/\">\uc81c\ubd84\uc18c \uc778\uc99d\uc11c<\/a> \uac15\ucca0\uacfc \ud568\uaed8 \uc774\ub3d9\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 id=\"h-related-reference-pages\" class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ud398\uc774\uc9c0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-annealing-normalizing-temperature-chart\/\">\uacf5\uad6c\uac15 \uc5b4\ub2d0\ub9c1 \ubc0f \ub178\uba40\ub77c\uc774\uc9d5 \uc628\ub3c4<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/d2-austenitizing-temperature\/\">D2 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-forging-temperature-guide\/\">\uacf5\uad6c\uac15 \ub2e8\uc870 \uc628\ub3c4 \uac00\uc774\ub4dc<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-machinability-rating-chart\/\">\uacf5\uad6c\uac15 \ud53c\uc0ad\uc131 \ub4f1\uae09<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/h13-steel-properties\/\">H13 \ub2e4\uc774\uce90\uc2a4\ud305 \uc801\uc6a9 \ubd84\uc57c<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel-machining-guide\/\">D2 \uacf5\uad6c\uac15 \uac00\uacf5 \uac00\uc774\ub4dc<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: Machinery\u2019s Handbook, 28th ed.(Industrial Press), \uacf5\uad6c\uac15 \ud45c 6, 8, 9, 10 \ubc0f \ud15c\ud37c \uc0c9\uc0c1\uc5d0 \uad00\ud55c \ud45c 1; ASM Handbook, Volume 1(10th ed.), Ultrahigh-Strength Steels, \ud45c 31 \ubc0f 33; Tool and Die Making Troubleshooter(R. M. Leed), \ud45c 8-3 \ubc0f 8-7; Heat Treatment, Selection and Application of Tool Steels(W. E. Bryson, 2nd ed.), \ud45c 10.1. \ucc38\uace0 \ub370\uc774\ud130\ub294 \ube44\uad50\uc6a9\uc785\ub2c8\ub2e4. \uc0dd\uc0b0 \uc804\uc5d0 \uc5f4\ucc98\ub9ac \uc5c5\uccb4 \ubc0f \uc81c\uac15\uc0ac \ub370\uc774\ud130 \uc2dc\ud2b8\ub85c \ud15c\ud37c\ub9c1 \uad00\ud589\uc744 \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>","protected":false},"excerpt":{"rendered":"<p>Tempering temperatures and the hardness they produce for common tool steels.<\/p>","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-18292","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Tool Steel Tempering Chart | Aobo Steel<\/title>\n<meta name=\"description\" content=\"Tempering temperatures and the hardness they produce for D2, D3, O1, A2, H13, M2, S7 and other common tool steels, with tempering colors in metric and imperial.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/tool-steel-tempering-chart\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Tempering temperature and working hardness\" \/>\n<meta property=\"og:description\" content=\"Tempering temperatures and the hardness they produce for D2, D3, O1, A2, H13, M2, S7 and other common tool steels, with tempering colors in metric and imperial.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/tool-steel-tempering-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-18T15:06:51+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"7\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-tempering-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-tempering-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Tempering temperature and working hardness\",\"datePublished\":\"2026-09-14T10:58:31+00:00\",\"dateModified\":\"2026-10-18T15:06:51+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-tempering-chart\\\/\"},\"wordCount\":1207,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-tempering-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-tempering-chart\\\/\",\"name\":\"Tool Steel Tempering Chart | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-14T10:58:31+00:00\",\"dateModified\":\"2026-10-18T15:06:51+00:00\",\"description\":\"Tempering temperatures and the hardness they produce for D2, D3, O1, A2, H13, M2, S7 and other common tool steels, with tempering colors in metric and imperial.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-tempering-chart\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-tempering-chart\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-tempering-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Tempering temperature and working hardness\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uacf5\uad6c\uac15 \ud15c\ud37c\ub9c1 \ucc28\ud2b8 | \uc544\ubcf4 \uc2a4\ud2f8","description":"D2, D3, O1, A2, H13, M2, S7 \ubc0f \uae30\ud0c0 \uc77c\ubc18 \uacf5\uad6c\uac15\uc758 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uc640 \uadf8\uc5d0 \ub530\ub978 \uacbd\ub3c4, \uadf8\ub9ac\uace0 \ud15c\ud37c\ub9c1 \uc0c9\uc0c1(\ubbf8\ud130\ubc95 \ubc0f \uc778\uce58\ubc95)\uc744 \ub098\ud0c0\ub0b8 \ud45c\uc785\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/tool-steel-tempering-chart\/","og_locale":"ko_KR","og_type":"article","og_title":"Tempering temperature and working hardness","og_description":"Tempering temperatures and the hardness they produce for D2, D3, O1, A2, H13, M2, S7 and other common tool steels, with tempering colors in metric and imperial.","og_url":"https:\/\/aobosteel.com\/ko\/tool-steel-tempering-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-18T15:06:51+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"7\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-tempering-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-tempering-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Tempering temperature and working hardness","datePublished":"2026-09-14T10:58:31+00:00","dateModified":"2026-10-18T15:06:51+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-tempering-chart\/"},"wordCount":1207,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-tempering-chart\/","url":"https:\/\/aobosteel.com\/tool-steel-tempering-chart\/","name":"\uacf5\uad6c\uac15 \ud15c\ud37c\ub9c1 \ucc28\ud2b8 | \uc544\ubcf4 \uc2a4\ud2f8","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-14T10:58:31+00:00","dateModified":"2026-10-18T15:06:51+00:00","description":"D2, D3, O1, A2, H13, M2, S7 \ubc0f \uae30\ud0c0 \uc77c\ubc18 \uacf5\uad6c\uac15\uc758 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uc640 \uadf8\uc5d0 \ub530\ub978 \uacbd\ub3c4, \uadf8\ub9ac\uace0 \ud15c\ud37c\ub9c1 \uc0c9\uc0c1(\ubbf8\ud130\ubc95 \ubc0f \uc778\uce58\ubc95)\uc744 \ub098\ud0c0\ub0b8 \ud45c\uc785\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-tempering-chart\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-tempering-chart\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-tempering-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Tempering temperature and working hardness"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tempering temperatures and the hardness they produce for common tool steels.","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tempering temperatures and the hardness they produce for common tool steels.","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18292","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=18292"}],"version-history":[{"count":25,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18292\/revisions"}],"predecessor-version":[{"id":23588,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18292\/revisions\/23588"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=18292"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}