{"id":18276,"date":"2026-09-14T11:37:47","date_gmt":"2026-09-14T03:37:47","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=18276"},"modified":"2026-10-20T09:01:53","modified_gmt":"2026-10-20T01:01:53","slug":"stainless-steel-physical-properties-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/stainless-steel-physical-properties-chart\/","title":{"rendered":"\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131 \ucc28\ud2b8"},"content":{"rendered":"<h1 class=\"wp-block-heading has-text-align-center\" id=\"h-stainless-steel-physical-properties-chart\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131 \ucc28\ud2b8<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">48\uc885\uc758 \uc555\uc5f0 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15(\uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc) \u2014 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uacc4, \ud398\ub77c\uc774\ud2b8\uacc4, \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4(410, 420, 440A, 440C) \ubc0f \uc11d\ucd9c\uacbd\ud654\uacc4 \u2014 \uc758 \ubc00\ub3c4, \ud0c4\uc131\uacc4\uc218, \uc5f4\ud33d\ucc3d, \uc5f4\uc804\ub3c4\ub3c4, \ube44\uc5f4, \uc804\uae30\uc800\ud56d \ubc0f \uc6a9\uc735 \ubc94\uc704. \ubbf8\ud130\ubc95 \uc218\uce58\uc640 \uc601\uad6d\uc2dd \ud658\uc0b0\uac12 \uc81c\uacf5.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\uc720\ud615<\/th><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">UNS<br>\ubc88\ud638<\/th><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\ubc00\ub3c4<br>g\/cm\u00b3<\/th><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\ud0c4\uc131<br>\uacc4\uc218<br>GPa<\/th><th class=\"has-text-align-left\" data-align=\"left\" colspan=\"3\">0 \u00b0C (32 \u00b0F)\uc5d0\uc11c\ubd80\ud130\uc758 \ud3c9\uade0 CTE<\/th><th class=\"has-text-align-left\" data-align=\"left\" colspan=\"2\">\uc5f4\uc804\ub3c4\uc728<\/th><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\ube44<br>\uc5f4 (a)<br>J\/kg\u00b7K<\/th><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\uc804\uae30<br>\uc800\ud56d\ub960<br>n\u03a9\u00b7m<\/th><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\uc790\uc11d<br>\ud22c\uc790\uc728 (b)<\/th><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\uc6a9\uc735 \ubc94\uc704<br>\u00b0C (\u00b0F)<\/th><\/tr><tr><th class=\"has-text-align-left\" data-align=\"left\">100 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">315 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">538 \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">100 \u00b0C\uc5d0\uc11c<\/th><th class=\"has-text-align-left\" data-align=\"left\">500 \u00b0C\uc5d0\uc11c<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">201<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20100<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">197 (28.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.7 (8.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.5 (9.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.4 (10.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">202<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20200<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.5 (9.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.4 (10.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.2 (10.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.6 (12.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20500<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">197 (28.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.9 (9.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.1 (10.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">301<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30100<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.2 (10.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1420 (2550-2590)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.8 (9.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.4 (10.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1420 (2550-2590)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">302B<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30215<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0 (10.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.4 (10.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.9 (9.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.6 (12.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1375-1400 (2550-2550)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">303<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30300<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.8 (9.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.4 (10.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2590)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.8 (9.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.4 (10.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">302Cu<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30430<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.8 (9.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.2 (6.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">304N<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30451<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">196 (28.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.8 (9.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.4 (10.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">308<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30800<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.8 (9.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.4 (10.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.2 (8.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.6 (12.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1420 (2550-2590)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">309<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30900<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.0 (8.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.6 (9.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.6 (9.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.7 (10.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">780<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31000<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.9 (8.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.2 (8.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.7 (10.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">780<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">314<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31400<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.1 (8.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.5 (10.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.9 (12.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">770<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31600<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.9 (8.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.5 (9.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">740<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1375-1400 (2500-2550)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1375-1400 (2500-2550)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316N<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31651<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">196 (28.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">740<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1375-1400 (2500-2550)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">317<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31700<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.9 (8.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.5 (9.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">740<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1375-1400 (2500-2550)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">317L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31703<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.5 (9.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.1 (10.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.4 (8.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">790<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1375-1400 (2500-2550)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">321<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32100<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.6 (9.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.6 (10.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.1 (9.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.2 (12.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1425 (2550-2600)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">329<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32900<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">750<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">330<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08330<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">196 (28.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.4 (8.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0 (8.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.7 (9.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1425 (2550-2600)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">347<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34700<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.6 (9.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.6 (10.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.1 (9.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.2 (12.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">730<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1425 (2550-2600)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">384<\/td><td class=\"has-text-align-left\" data-align=\"left\">S38400<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0 (0.29)<\/td><td class=\"has-text-align-left\" data-align=\"left\">193 (28.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.2 (9.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.8 (9.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.4 (10.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.2 (9.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5 (12.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450 (2550-2650)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">405<\/td><td class=\"has-text-align-left\" data-align=\"left\">S40500<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.8 (6.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.6 (6.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.1 (6.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.0 (15.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1480-1530 (2700-2790)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">409<\/td><td class=\"has-text-align-left\" data-align=\"left\">S40900<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.7 (6.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1480-1530 (2700-2790)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">410<\/td><td class=\"has-text-align-left\" data-align=\"left\">S41000<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.9 (5.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.4 (6.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.6 (6.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.9 (14.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.7 (16.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">570<\/td><td class=\"has-text-align-left\" data-align=\"left\">700-1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">1480-1530 (2700-2790)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">414<\/td><td class=\"has-text-align-left\" data-align=\"left\">S41400<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.4 (5.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0 (6.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.1 (6.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.9 (14.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.7 (16.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">700<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1425-1480 (2600-2700)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">416<\/td><td class=\"has-text-align-left\" data-align=\"left\">S41600<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.9 (5.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0 (6.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.6 (6.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.9 (14.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.7 (16.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">570<\/td><td class=\"has-text-align-left\" data-align=\"left\">700-1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">1480-1530 (2700-2790)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">420<\/td><td class=\"has-text-align-left\" data-align=\"left\">S42000<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.3 (5.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.8 (6.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.7 (6.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.9 (14.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1510 (2650-2750)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">422<\/td><td class=\"has-text-align-left\" data-align=\"left\">S42200<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.2 (6.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.4 (6.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.9 (6.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.9 (13.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.3 (15.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1470-1480 (2675-2700)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">429<\/td><td class=\"has-text-align-left\" data-align=\"left\">S42900<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.3 (5.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.6 (14.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">590<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1510 (2650-2750)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">430<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43000<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.4 (5.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0 (6.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.4 (6.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.1 (15.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.3 (15.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">600-1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">1425-1510 (2600-2750)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">430F<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43020<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.4 (5.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0 (6.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.4 (6.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.1 (15.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.3 (15.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1425-1510 (2600-2750)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">431<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43100<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.2 (5.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.1 (6.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.2 (11.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">720<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">434<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43400<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.4 (5.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0 (6.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.4 (6.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.3 (15.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">600-1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">1425-1510 (2600-2750)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">436<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43600<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.3 (5.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.9 (13.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.0 (15.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">600-1100<\/td><td class=\"has-text-align-left\" data-align=\"left\">1425-1510 (2600-2750)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">439<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43035<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.7 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.4 (5.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0 (6.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.4 (6.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.2 (14.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">630<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/440a-stainless-steel-heat-treatment\/\">440A<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">S44002<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.2 (5.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.2 (14.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1370-1480 (2500-2700)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">440C<\/td><td class=\"has-text-align-left\" data-align=\"left\">S44004<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.2 (5.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.2 (14.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1370-1480 (2500-2700)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">444<\/td><td class=\"has-text-align-left\" data-align=\"left\">S44400<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0 (5.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.6 (5.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.4 (6.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.8 (15.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">420 (0.10)<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">446<\/td><td class=\"has-text-align-left\" data-align=\"left\">S44600<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.5 (0.27)<\/td><td class=\"has-text-align-left\" data-align=\"left\">200 (29.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.4 (5.8)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.8 (6.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.2 (6.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.9 (12.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.4 (14.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">500 (0.12)<\/td><td class=\"has-text-align-left\" data-align=\"left\">670<\/td><td class=\"has-text-align-left\" data-align=\"left\">400-700<\/td><td class=\"has-text-align-left\" data-align=\"left\">1425-1510 (2600-2750)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PH 13-8 Mo<\/td><td class=\"has-text-align-left\" data-align=\"left\">S13800<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">203 (29.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.6 (5.9)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.2 (6.2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.9 (6.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.0 (8.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.0 (12.7)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1440 (2560-2625)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">15-5 PH<\/td><td class=\"has-text-align-left\" data-align=\"left\">S15500<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">196 (28.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.8 (6.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.4 (6.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.8 (10.3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.0 (13.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">420 (0.10)<\/td><td class=\"has-text-align-left\" data-align=\"left\">770<\/td><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1440 (2560-2625)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">17-4 PH<\/td><td class=\"has-text-align-left\" data-align=\"left\">S17400<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">196 (28.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.8 (6.0)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.6 (6.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.3 (10.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.0 (13.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">800<\/td><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1440 (2560-2625)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">17-7 PH<\/td><td class=\"has-text-align-left\" data-align=\"left\">S17700<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.8 (0.28)<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 (29.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0 (6.1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.6 (6.4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.4 (9.5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.8 (12.6)<\/td><td class=\"has-text-align-left\" data-align=\"left\">460 (0.11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">830<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1440 (2560-2625)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<ul class=\"wp-block-list\">\n<li><sup>(a)<\/sup> 0~100 \u00b0C (32~212 \u00b0F)\uc5d0\uc11c.<\/li>\n\n\n\n<li><sup>(b)<\/sup> \uadfc\uc0ac\uac12.<\/li>\n\n\n\n<li>CTE, \uc5f4\ud33d\ucc3d \uacc4\uc218.<\/li>\n<\/ul>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131 \ucc28\ud2b8, \uc778\uc1c4 \uac00\ub2a5\ud55c PDF<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">48\uac1c \ub4f1\uae09\uc758 \ubc00\ub3c4, \ud0c4\uc131\uacc4\uc218, \uc5f4\ud33d\ucc3d, \uc5f4\uc804\ub3c4\uc728, \ube44\uc5f4, \uc804\uae30 \uc800\ud56d\ub960, \ud22c\uc790\uc728, \uc6a9\uc735 \ubc94\uc704\ub97c \ub2f4\uc740 \uc778\uc1c4\uc6a9 PDF\uc785\ub2c8\ub2e4. \uc5f0\ub77d\ucc98\uac00 \ud568\uaed8 \ub4e4\uc5b4 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Stainless-Steel-Physical-Properties-Chart.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc, 587 KB<\/a><\/div>\n<\/div>\n<\/div>\n\n\n\n<h3 id=\"h-table-notes\" class=\"wp-block-heading\">\ud14c\uc774\ube14 \ub178\ud2b8<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc\uc758 \ub2e8\uc870 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc758 \ub300\ud45c\uc801 \ubb3c\ub9ac\uc801 \ud2b9\uc131: \ubc00\ub3c4, \ud0c4\uc131\uacc4\uc218, \ud3c9\uade0 \uc5f4\ud33d\ucc3d\uacc4\uc218(CTE), \uc5f4\uc804\ub3c4\uc728, \ube44\uc5f4, \uc804\uae30\uc800\ud56d\ub960, \ud22c\uc790\uc728 \ubc0f \uc6a9\uc735 \ubc94\uc704. \uac12\uc740 \ubbf8\ud130\ubc95 \ub2e8\uc704\ub85c \uc81c\uc2dc\ud558\uba70, \ucd9c\ucc98\uc758 \uc57c\ub4dc\ud30c\uc6b4\ub4dc\ubc95 \ud658\uc0b0\uac12\uc744 \uad04\ud638 \uc548\uc5d0 \ubcd1\uae30\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">CTE\ub294 0 \u00b0C (32 \u00b0F)\uc5d0\uc11c \ud45c\uae30\ub41c \uc628\ub3c4\uae4c\uc9c0\uc758 \ud3c9\uade0 \uacc4\uc218\uc774\uba70, \uc5f4\uc804\ub3c4\uc728\uc740 100 \u00b0C \ubc0f 500 \u00b0C\uc5d0\uc11c \ud45c\uae30\ub429\ub2c8\ub2e4. \uc774\ub294 \uacf5\uad6c, \uae08\ud615 \ubc0f \uc9c0\uadf8\uc758 \uc5f4\ud33d\ucc3d \ubc0f \uc5f4\uc804\ub2ec \uacc4\uc0b0\uacfc \uc77c\ubc18 \uc124\uacc4 \uc791\uc5c5\uc5d0 \uc0ac\uc6a9\ub418\ub294 \uc785\ub825\uac12\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>\uba54\ubaa8:<\/strong> \ucd9c\ucc98\uc5d0\uc11c \ub450 \uac1c\uc758 \uc6a9\uc735 \ubc94\uc704\uac00 \uc77c\uad00\uc131 \uc5c6\uc774 \uc778\uc1c4\ub418\uc5b4 \uc788\uc73c\uba70 \ud45c\uae30\ub41c \uadf8\ub300\ub85c \uc7ac\ud604\ud569\ub2c8\ub2e4: type 302B, 1375\u20131400 \u00b0C (2550\u20132550 \u00b0F), \ubc0f type 303, 1400\u20131450 \u00b0C (2550\u20132590 \u00b0F).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc790\uae30 \ud22c\uc790\uc728\uc740 \uadfc\uc0ac\uac12\uc774\uba70, \ud398\ub77c\uc774\ud2b8\uacc4 \ubc0f \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4(405, 410, 420, 430, 440A, 440C \ub4f1)\ub294 \uc790\uc131\uc774 \uc788\uace0 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uacc4\ub294 \ubcf8\uc9c8\uc801\uc73c\ub85c \ube44\uc790\uc131(\uac12 1.02)\uc785\ub2c8\ub2e4. \uc124\uacc4 \uc0ac\uc6a9 \uc804\uc5d0 \ud574\ub2f9 \uc81c\ud488 \uc0ac\uc591\uacfc \ub300\uc870\ud558\uc5ec \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<h3 id=\"h-related-reference-pages\" class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ud398\uc774\uc9c0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"\/ko\/stainless-steel-composition-chart\/\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uc131\ubd84\ud45c<\/a> \u00b7 <a href=\"\/ko\/martensitic-stainless-steel-properties-chart\/\">\ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uae30\uacc4\uc801 \ud2b9\uc131<\/a> \u00b7 <a href=\"\/ko\/420-stainless-steel\/\">420 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15<\/a> \u00b7 <a href=\"\/ko\/440c-stainless-steel\/\">440C \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15<\/a> \u00b7 <a href=\"\/ko\/440c-stainless-steel-properties\/\">440C \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15 \ud2b9\uc131<\/a> \u00b7 <a href=\"\/ko\/4cr13-stainless-steel\/\">4Cr13 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15<\/a> \u00b7 <a href=\"\/ko\/stainless-steels\/\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uac1c\uc694<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Volume 1 \u2014 Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 21 \u201cTypical physical properties of wrought stainless steels, annealed condition\u201d (10th ed., pp. 2102\u20132106). \ube44\uad50\uc6a9 \ucc38\uc870 \ub370\uc774\ud130 \u2014 \uc124\uacc4\uc5d0 \uc0ac\uc6a9\ud558\uae30 \uc804\uc5d0 \ud574\ub2f9 \uc81c\ud488 \uc0ac\uc591\uacfc \ub300\uc870\ud558\uc5ec \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>","protected":false},"excerpt":{"rendered":"<p>Stainless Steel Physical Properties Chart Density, elastic modulus, thermal expansion, thermal conductivity, specific heat, electrical resistivity and melting range for 48 wrought stainless steels in the annealed condition \u2014 austenitic, ferritic, martensitic (410, 420, 440A, 440C) and precipitation-hardening types. Metric values with imperial equivalents. Type UNSnumber Densityg\/cm\u00b3 ElasticmodulusGPa Mean CTE from 0 \u00b0C (32 \u00b0F) [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-18276","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Stainless Steel Physical Properties Chart - AoboSteel<\/title>\n<meta name=\"description\" content=\"Density, thermal expansion, conductivity, elastic modulus and melting range for 48 stainless steels \u2014 420, 440C, 410, 304, 316 and 17-4 PH. Metric and imperial.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/stainless-steel-physical-properties-chart\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Stainless Steel Physical Properties Chart\" \/>\n<meta property=\"og:description\" content=\"Density, thermal expansion, conductivity, elastic modulus and melting range for 48 stainless steels \u2014 420, 440C, 410, 304, 316 and 17-4 PH. Metric and imperial.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/stainless-steel-physical-properties-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-20T01:01:53+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"6\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-physical-properties-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-physical-properties-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Stainless Steel Physical Properties Chart\",\"datePublished\":\"2026-09-14T03:37:47+00:00\",\"dateModified\":\"2026-10-20T01:01:53+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-physical-properties-chart\\\/\"},\"wordCount\":497,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-physical-properties-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-physical-properties-chart\\\/\",\"name\":\"Stainless Steel Physical Properties Chart - AoboSteel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-14T03:37:47+00:00\",\"dateModified\":\"2026-10-20T01:01:53+00:00\",\"description\":\"Density, thermal expansion, conductivity, elastic modulus and melting range for 48 stainless steels \u2014 420, 440C, 410, 304, 316 and 17-4 PH. Metric and imperial.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-physical-properties-chart\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-physical-properties-chart\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-physical-properties-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Stainless Steel Physical Properties Chart\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131 \ucc28\ud2b8 - AoboSteel","description":"48\uac1c \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15\uc758 \ubc00\ub3c4, \uc5f4\ud33d\ucc3d, \uc5f4\uc804\ub3c4\uc728, \ud0c4\uc131\uacc4\uc218, \uc6a9\uc735 \ubc94\uc704. 420, 440C, 410, 304, 316, 17-4 PH. \ubbf8\ud130\ubc95\uacfc \uc778\uce58 \ub2e8\uc704.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/stainless-steel-physical-properties-chart\/","og_locale":"ko_KR","og_type":"article","og_title":"Stainless Steel Physical Properties Chart","og_description":"Density, thermal expansion, conductivity, elastic modulus and melting range for 48 stainless steels \u2014 420, 440C, 410, 304, 316 and 17-4 PH. Metric and imperial.","og_url":"https:\/\/aobosteel.com\/ko\/stainless-steel-physical-properties-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-20T01:01:53+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"6\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/stainless-steel-physical-properties-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/stainless-steel-physical-properties-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Stainless Steel Physical Properties Chart","datePublished":"2026-09-14T03:37:47+00:00","dateModified":"2026-10-20T01:01:53+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/stainless-steel-physical-properties-chart\/"},"wordCount":497,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/stainless-steel-physical-properties-chart\/","url":"https:\/\/aobosteel.com\/stainless-steel-physical-properties-chart\/","name":"\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131 \ucc28\ud2b8 - AoboSteel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-14T03:37:47+00:00","dateModified":"2026-10-20T01:01:53+00:00","description":"48\uac1c \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15\uc758 \ubc00\ub3c4, \uc5f4\ud33d\ucc3d, \uc5f4\uc804\ub3c4\uc728, \ud0c4\uc131\uacc4\uc218, \uc6a9\uc735 \ubc94\uc704. 420, 440C, 410, 304, 316, 17-4 PH. \ubbf8\ud130\ubc95\uacfc \uc778\uce58 \ub2e8\uc704.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/stainless-steel-physical-properties-chart\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/stainless-steel-physical-properties-chart\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/stainless-steel-physical-properties-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Stainless Steel Physical Properties Chart"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Stainless Steel Physical Properties Chart Density, elastic modulus, thermal expansion, thermal conductivity, specific heat, electrical resistivity and melting range for 48 wrought stainless steels in the annealed condition \u2014 austenitic, ferritic, martensitic (410, 420, 440A, 440C) and precipitation-hardening types. Metric values with imperial equivalents. Type UNSnumber Densityg\/cm\u00b3 ElasticmodulusGPa Mean CTE from 0 \u00b0C (32 \u00b0F)&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Stainless Steel Physical Properties Chart Density, elastic modulus, thermal expansion, thermal conductivity, specific heat, electrical resistivity and melting range for 48 wrought stainless steels in the annealed condition \u2014 austenitic, ferritic, martensitic (410, 420, 440A, 440C) and precipitation-hardening types. Metric values with imperial equivalents. Type UNSnumber Densityg\/cm\u00b3 ElasticmodulusGPa Mean CTE from 0 \u00b0C (32 \u00b0F)&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18276","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=18276"}],"version-history":[{"count":10,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18276\/revisions"}],"predecessor-version":[{"id":23758,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18276\/revisions\/23758"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=18276"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}