{"id":18254,"date":"2026-09-13T20:57:17","date_gmt":"2026-09-13T12:57:17","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=18254"},"modified":"2026-10-16T16:39:49","modified_gmt":"2026-10-16T08:39:49","slug":"martensitic-stainless-steel-properties-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/martensitic-stainless-steel-properties-chart\/","title":{"rendered":"\ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ud2b9\uc131 \ucc28\ud2b8 (403-440C)"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ud2b9\uc131 \ucc28\ud2b8<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\ud45c\uc900 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 403\ubd80\ud130 440C\uae4c\uc9c0\uc758 \ucd5c\uc18c \uae30\uacc4\uc801 \ud2b9\uc131\uc73c\ub85c, \ucf8c\uc0ad\uac15 \ubc0f \ud2b9\uc218 \uc720\ud615\uc744 \ud3ec\ud568\ud569\ub2c8\ub2e4. \ud589\uc740 \uc720\ud615\ubcc4\ub85c \uadf8\ub8f9\ud654\ub418\uc5b4 \uc788\uc73c\uba70, \uac01 \ud589\uc740 \uc81c\ud488 \ud615\ud0dc\uc640 \uc0c1\ud0dc\uc5d0 \ub530\ub978 \uc778\uc7a5 \uac15\ub3c4, \ud56d\ubcf5 \uac15\ub3c4, \uc5f0\uc2e0\uc728, \uacbd\ub3c4 \ubc0f \ud574\ub2f9 ASTM \uaddc\uaca9\uc744 \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>MPa \/ ksi<\/strong> \ub3d9\uc77c \uac12, \ub450 \ub2e8\uc704<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>(a)\u2013(d)<\/strong> \uac01\uc8fc<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>(c)<\/strong> \uc77c\ubc18\uc801\uc778 \uac12<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>&mdash;<\/strong> \uba85\uc2dc\ub418\uc9c0 \uc54a\uc74c<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud615\ud0dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\ud0dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc778\uc7a5\ub825<br>MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">0.2% \ud56d\ubcf5<br>MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc7a5<br>%<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub2e8\uba74 \uc218\ucd95\ub960<br>%<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">ASTM \uaddc\uaca9<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 403 (UNS S40300)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \uc5f4\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473, A 479<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \uc5f4\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\uc9c8 \ub728\uc784, \uc5f4\uac04 \ub610\ub294 \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">825<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\uc9c8 \ub728\uc784, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">825<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">25 <sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">88 HRB \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 176<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">\uc720\ud615 <a href=\"https:\/\/aobosteel.com\/ko\/410-stainless-steel-heat-treatment\/\">410<\/a> (UNS S41000)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \uc5f4\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473, A 479<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \uc5f4\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\uc9c8 \ub728\uc784, \uc5f4\uac04 \ub610\ub294 \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">825<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\uc9c8 \ub728\uc784, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">825<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">22 <sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 176<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 410S (UNS S41008)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">415<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">22 <sup>(b)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">88 HRB \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 176, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 410Cb (UNS S41040)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \uc5f4\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 479<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 479<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \uc5f4\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">860<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, 479<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">860<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 479<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">E-4 (UNS S41050)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">415<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">88 HRB \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 414 (UNS S41400)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784, \ub0c9\uac04 \ub610\ub294 \uc5f4\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">795<\/td><td class=\"has-text-align-left\" data-align=\"left\">115<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 479<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">1030 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">150 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">CA6NM (UNS S41500)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub4dc<\/td><td class=\"has-text-align-left\" data-align=\"left\">795<\/td><td class=\"has-text-align-left\" data-align=\"left\">115<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">32 HRC \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 176, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub4dc<\/td><td class=\"has-text-align-left\" data-align=\"left\">795<\/td><td class=\"has-text-align-left\" data-align=\"left\">115<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473, A 479<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">\uc720\ud615 <a href=\"https:\/\/aobosteel.com\/ko\/416-stainless-steel-heat-treatment\/\">416<\/a> (UNS S41600) \ubc0f 416Se (UNS S41623)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">585-860<\/td><td class=\"has-text-align-left\" data-align=\"left\">85-125<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">795-1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">115-145<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\uc9c8 \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">965-1210<\/td><td class=\"has-text-align-left\" data-align=\"left\">140-175<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 416 plus X (UNS S41610)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">585-860<\/td><td class=\"has-text-align-left\" data-align=\"left\">85-125<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">795-1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">115-145<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\uc9c8 \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">965-1210<\/td><td class=\"has-text-align-left\" data-align=\"left\">140-175<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 418 (UNS S41800)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">620 \u00b0C (1150 \u00b0F)\uc5d0\uc11c \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">965<\/td><td class=\"has-text-align-left\" data-align=\"left\">140<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 565<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 420 (UNS S42000)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 \u00b0C (400 \u00b0F)\uc5d0\uc11c \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">1720<\/td><td class=\"has-text-align-left\" data-align=\"left\">250<\/td><td class=\"has-text-align-left\" data-align=\"left\">1480 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">215 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">8 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">25 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">52 HRC <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">860 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">125 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 176<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">TrimRite (UNS S42010)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">690 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 493<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub7c9 \ub4dc\ub798\ud504\ud2b8<\/td><td class=\"has-text-align-left\" data-align=\"left\">725 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">105 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 493<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 422 (UNS S42200)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">675 \u00b0C (1250 \u00b0F)\uc5d0\uc11c \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">825<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">585<\/td><td class=\"has-text-align-left\" data-align=\"left\">85<\/td><td class=\"has-text-align-left\" data-align=\"left\">17 <sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 565<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">620 \u00b0C (1150 \u00b0F)\uc5d0\uc11c \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">965<\/td><td class=\"has-text-align-left\" data-align=\"left\">140<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 565<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Lapelloy (UNS S42300)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">620 \u00b0C (1150 \u00b0F)\uc5d0\uc11c \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">965<\/td><td class=\"has-text-align-left\" data-align=\"left\">140<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 565<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 431 (UNS S43100)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">795<\/td><td class=\"has-text-align-left\" data-align=\"left\">115<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\uc9c8 \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">1210<\/td><td class=\"has-text-align-left\" data-align=\"left\">175<\/td><td class=\"has-text-align-left\" data-align=\"left\">930<\/td><td class=\"has-text-align-left\" data-align=\"left\">135<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">965 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">140 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 493<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub7c9 \ub4dc\ub798\ud504\ud2b8<\/td><td class=\"has-text-align-left\" data-align=\"left\">795<\/td><td class=\"has-text-align-left\" data-align=\"left\">115<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 493<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 440A (UNS S44002)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">725 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">105 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">415 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">60 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">20 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">315 \u00b0C (600 \u00b0F)\uc5d0\uc11c \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">1790 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">260 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">1650 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">240 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">5 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">20 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">51 HRC <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">965 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">140 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">\uc720\ud615 <a href=\"https:\/\/aobosteel.com\/ko\/440b-stainless-steel-heat-treatment\/\">440B<\/a> (UNS S44003)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">740 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">107 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">425 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">62 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">18 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">315 \u00b0C (600 \u00b0F)\uc5d0\uc11c \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">1930 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">280 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">1860 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">270 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">3 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">15 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">55 HRC <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">965 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">140 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Type 440C (UNS S44004)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1\ub41c<\/td><td class=\"has-text-align-left\" data-align=\"left\">760 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">110 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">450 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">65 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">14 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">97 HRB <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">315 \u00b0C (600 \u00b0F)\uc5d0\uc11c \ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">1970 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">285 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">1900 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">275 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">2 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">10 <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">57 HRC <sup>(c)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud480\ub9bc, \ub0c9\uac04 \ub9c8\ubb34\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">965 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">140 \ucd5c\ub300<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<ul class=\"wp-block-list\">\n<li><sup>(a)<\/sup> B, \ubd09\uc7ac; F, \ub2e8\uc870\ud488; P, \ud310\uc7ac; Sh, \uc2dc\ud2b8; St, \uc2a4\ud2b8\ub9bd; W, \uc640\uc774\uc5b4.<\/li>\n\n<li><sup>(b)<\/sup> \ub450\uaed8 1.3 mm (0.050 in.) \uc774\ud558\uc758 \uacbd\uc6b0 \uc5f0\uc2e0\uc728 20%.<\/li>\n\n<li><sup>(c)<\/sup> \uc77c\ubc18\uc801\uc778 \uac12.<\/li>\n\n<li><sup>(d)<\/sup> \ub2e8\uc870\ud488\uc758 \uacbd\uc6b0 \ucd5c\uc18c \uc5f0\uc2e0\uc728 15%.<\/li>\n<\/ul>\n\n\n\n<h3 class=\"wp-block-heading\">\ud14c\uc774\ube14 \ub178\ud2b8<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\ud45c\uc900 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15\uc885\uc758 \ucd5c\uc18c \uae30\uacc4\uc801 \ud2b9\uc131\uc73c\ub85c, \uac15\uc885\ubcc4\ub85c \ubd84\ub958\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. \uac01 \ud589\uc740 \uc81c\ud488 \ud615\ud0dc\uc640 \uc0c1\ud0dc\ub97c \ud574\ub2f9 \uc0c1\ud0dc\uc5d0\uc11c \ubcf4\uc99d\ub418\uac70\ub098 \uc77c\ubc18\uc801\uc73c\ub85c \uc608\uc0c1\ub418\ub294 \ud2b9\uc131\uacfc \uc5f0\uacb0\ud569\ub2c8\ub2e4. MPa \ubc0f ksi \uc5f4\uc740 \ub3d9\uc77c\ud55c \uac12\uc744 \ub450 \ub2e8\uc704\ub85c \ub098\ud0c0\ub0b8 \uac83\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uacbd\ub3c4\ub294 \uc778\uc1c4\ub41c \uadf8\ub300\ub85c \ub85d\uc6f0 B, \ub85d\uc6f0 C \ub610\ub294 \ube0c\ub9ac\ub12c\ub85c \ud45c\uc2dc\ub418\uba70, (c) \uac12\uc740 \ubcf4\uc99d \ucd5c\uc18c\uac12\uc774 \uc544\ub2cc \uc77c\ubc18\uc801\uc778 \uac12\uc785\ub2c8\ub2e4. \uaddc\uaca9 \uc5f4\uc5d0\ub294 \uac01 \ud589\uc774 \uc778\uc6a9\ub41c ASTM \uaddc\uaca9(A 276, A 473, A 479, A 580, A 581 \ub4f1)\uc774 \ub098\uc5f4\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc6d0\ubb38\uc5d0\uc11c \ud55c \uaddc\uaca9 \uc140\uc740 &ldquo;A 276, 479&rdquo;\ub85c \ud45c\uae30\ub418\uc5b4 \uc788\uc73c\uba70, \uc5ec\uae30\uc11c\ub294 A 276, A 479\ub85c \uc77d\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ube44\uad50\uc6a9 \ucc38\uace0 \ub370\uc774\ud130 &mdash; \uc8fc\ubb38 \ub610\ub294 \uc124\uacc4 \uc804\uc5d0 \uc801\uc6a9 \uac00\ub2a5\ud55c \uaddc\uaca9\uacfc \ub9c8\uac10 \uc0c1\ud0dc\ub97c \ubc00 \uc778\uc99d\uc11c\uc5d0\uc11c \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\uad00\ub828 \ucc38\uc870 \ud398\uc774\uc9c0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"\/ko\/420-stainless-steel\/\">420 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15<\/a> \u00b7 <a href=\"\/ko\/440c-stainless-steel\/\">440C \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15<\/a> \u00b7 <a href=\"\/ko\/440c-stainless-steel-properties\/\">440C \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15 \ud2b9\uc131<\/a> \u00b7 <a href=\"\/ko\/4cr13-stainless-steel\/\">4Cr13 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15<\/a> \u00b7 <a href=\"\/ko\/stainless-steel-composition-chart\/\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uc131\ubd84\ud45c<\/a> \u00b7 <a href=\"\/ko\/420-stainless-steel-heat-treatment\/\">420 \uc5f4\ucc98\ub9ac<\/a> \u00b7 <a href=\"\/ko\/440c-stainless-steel-heat-treatment\/\">440C \uc5f4\ucc98\ub9ac<\/a> \u00b7 <a href=\"\/ko\/9cr18mo-stainless-steel\/\">9Cr18Mo \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15<\/a> \u00b7 <a href=\"\/ko\/stainless-steels\/\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uac1c\uc694<\/a> \u00b7 <a href=\"\/ko\/d2-steel-vs-440c\/\">D2 \uac15 \ub300 440C<\/a> \u00b7 <a href=\"\/ko\/stainless-steel-physical-properties-chart\/\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ubb3c\ub9ac\uc801 \ud2b9\uc131 \ucc28\ud2b8<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Volume 1 &mdash; Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 11 &ldquo;Minimum mechanical properties of martensitic stainless steels&rdquo; (10th ed.). \ube44\uad50\uc6a9 \ucc38\uace0 \ub370\uc774\ud130 &mdash; \uc8fc\ubb38 \uc804\uc5d0 \uc801\uc6a9 \uac00\ub2a5\ud55c \ud45c\uc900\uc744 \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>","protected":false},"excerpt":{"rendered":"<p>Martensitic Stainless Steel Properties Chart Minimum mechanical properties of the standard martensitic stainless steels &mdash; 403 through 440C, including the free-machining and specialty types. Rows are grouped by type; each row gives a product form and condition with its tensile strength, yield strength, elongation, hardness and governing ASTM specification. MPa \/ ksi same value, two [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-18254","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Martensitic Stainless Steel Properties Chart (403-440C) - AoboSteel<\/title>\n<meta name=\"description\" content=\"Minimum mechanical properties of martensitic stainless steels 403, 410, 416, 420, 431, 440A, 440B and 440C \u2014 tensile and yield strength, elongation, hardness by product form, condition and ASTM spec.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/martensitic-stainless-steel-properties-chart\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Martensitic Stainless Steel Properties Chart (403-440C)\" \/>\n<meta property=\"og:description\" content=\"Minimum mechanical properties of martensitic stainless steels 403, 410, 416, 420, 431, 440A, 440B and 440C \u2014 tensile and yield strength, elongation, hardness by product form, condition and ASTM spec.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/martensitic-stainless-steel-properties-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-16T08:39:49+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"6\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/martensitic-stainless-steel-properties-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/martensitic-stainless-steel-properties-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Martensitic Stainless Steel Properties Chart (403-440C)\",\"datePublished\":\"2026-09-13T12:57:17+00:00\",\"dateModified\":\"2026-10-16T08:39:49+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/martensitic-stainless-steel-properties-chart\\\/\"},\"wordCount\":801,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/martensitic-stainless-steel-properties-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/martensitic-stainless-steel-properties-chart\\\/\",\"name\":\"Martensitic Stainless Steel Properties Chart (403-440C) - AoboSteel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-13T12:57:17+00:00\",\"dateModified\":\"2026-10-16T08:39:49+00:00\",\"description\":\"Minimum mechanical properties of martensitic stainless steels 403, 410, 416, 420, 431, 440A, 440B and 440C \u2014 tensile and yield strength, elongation, hardness by product form, condition and ASTM spec.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/martensitic-stainless-steel-properties-chart\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/martensitic-stainless-steel-properties-chart\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/martensitic-stainless-steel-properties-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Martensitic Stainless Steel Properties Chart (403-440C)\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ud2b9\uc131 \ucc28\ud2b8 (403-440C) - AoboSteel","description":"\ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 403, 410, 416, 420, 431, 440A, 440B, 440C\uc758 \ucd5c\uc18c \uae30\uacc4\uc801 \uc131\uc9c8 \u2014 \uc81c\ud488 \ud615\ud0dc, \uc0c1\ud0dc, ASTM \uaddc\uaca9\ubcc4 \uc778\uc7a5 \uac15\ub3c4, \ud56d\ubcf5 \uac15\ub3c4, \uc5f0\uc2e0\uc728, \uacbd\ub3c4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/martensitic-stainless-steel-properties-chart\/","og_locale":"ko_KR","og_type":"article","og_title":"Martensitic Stainless Steel Properties Chart (403-440C)","og_description":"Minimum mechanical properties of martensitic stainless steels 403, 410, 416, 420, 431, 440A, 440B and 440C \u2014 tensile and yield strength, elongation, hardness by product form, condition and ASTM spec.","og_url":"https:\/\/aobosteel.com\/ko\/martensitic-stainless-steel-properties-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-16T08:39:49+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"6\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/martensitic-stainless-steel-properties-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/martensitic-stainless-steel-properties-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Martensitic Stainless Steel Properties Chart (403-440C)","datePublished":"2026-09-13T12:57:17+00:00","dateModified":"2026-10-16T08:39:49+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/martensitic-stainless-steel-properties-chart\/"},"wordCount":801,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/martensitic-stainless-steel-properties-chart\/","url":"https:\/\/aobosteel.com\/martensitic-stainless-steel-properties-chart\/","name":"\ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ud2b9\uc131 \ucc28\ud2b8 (403-440C) - AoboSteel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-13T12:57:17+00:00","dateModified":"2026-10-16T08:39:49+00:00","description":"\ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 403, 410, 416, 420, 431, 440A, 440B, 440C\uc758 \ucd5c\uc18c \uae30\uacc4\uc801 \uc131\uc9c8 \u2014 \uc81c\ud488 \ud615\ud0dc, \uc0c1\ud0dc, ASTM \uaddc\uaca9\ubcc4 \uc778\uc7a5 \uac15\ub3c4, \ud56d\ubcf5 \uac15\ub3c4, \uc5f0\uc2e0\uc728, \uacbd\ub3c4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/martensitic-stainless-steel-properties-chart\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/martensitic-stainless-steel-properties-chart\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/martensitic-stainless-steel-properties-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Martensitic Stainless Steel Properties Chart (403-440C)"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Martensitic Stainless Steel Properties Chart Minimum mechanical properties of the standard martensitic stainless steels &mdash; 403 through 440C, including the free-machining and specialty types. Rows are grouped by type; each row gives a product form and condition with its tensile strength, yield strength, elongation, hardness and governing ASTM specification. MPa \/ ksi same value, two&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Martensitic Stainless Steel Properties Chart Minimum mechanical properties of the standard martensitic stainless steels &mdash; 403 through 440C, including the free-machining and specialty types. Rows are grouped by type; each row gives a product form and condition with its tensile strength, yield strength, elongation, hardness and governing ASTM specification. MPa \/ ksi same value, two&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18254","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=18254"}],"version-history":[{"count":11,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18254\/revisions"}],"predecessor-version":[{"id":23242,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/18254\/revisions\/23242"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=18254"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}