{"id":13401,"date":"2026-03-10T11:09:23","date_gmt":"2026-03-10T03:09:23","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=13401"},"modified":"2026-06-04T08:43:04","modified_gmt":"2026-06-04T00:43:04","slug":"d2-tool-steel-machining-parameters","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/d2-tool-steel-machining-parameters\/","title":{"rendered":"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding"},"content":{"rendered":"<section class=\"aobo-d2-machining-page\">\n  <style>\n    .aobo-d2-machining-page {\n      --aobo-blue: #0c56d0;\n      --aobo-blue-dark: #073b8e;\n      --aobo-blue-soft: #eaf2ff;\n      --aobo-border: #d7e5fb;\n      --aobo-text: #203044;\n      --aobo-muted: #617087;\n      --aobo-orange: #f59b23;\n      --aobo-white: #ffffff;\n      --aobo-shadow: 0 18px 45px rgba(12, 86, 208, 0.10);\n      --aobo-page-width: 1180px;\n      font-family: Arial, Helvetica, sans-serif;\n      color: var(--aobo-text);\n      line-height: 1.7;\n      background: transparent;\n      padding: 0;\n      box-sizing: border-box;\n    }\n\n    .aobo-d2-machining-page * {\n      box-sizing: border-box;\n    }\n\n    .aobo-wrap {\n      max-width: var(--aobo-page-width);\n      margin: 0 auto;\n      padding: 0;\n    }\n\n    .aobo-hero {\n      background: linear-gradient(135deg, #ffffff 0%, #f7fbff 58%, #eaf2ff 100%);\n      border: 1px solid var(--aobo-border);\n      border-radius: 26px;\n      padding: 42px 38px;\n      margin-bottom: 30px;\n      box-shadow: var(--aobo-shadow);\n      overflow: hidden;\n      position: relative;\n    }\n\n    .aobo-hero::after {\n      content: \"\";\n      position: absolute;\n      right: -90px;\n      top: -90px;\n      width: 260px;\n      height: 260px;\n      border-radius: 50%;\n      background: rgba(12, 86, 208, 0.08);\n    }\n\n    .aobo-eyebrow {\n      display: inline-block;\n      margin-bottom: 12px;\n      padding: 6px 12px;\n      border-radius: 999px;\n      background: #fff7ed;\n      border: 1px solid #fde3bd;\n      color: var(--aobo-orange);\n      font-size: 14px;\n      font-weight: 700;\n      position: relative;\n      z-index: 2;\n    }\n\n    .aobo-hero h1 {\n      margin: 0 0 16px;\n      color: #082d6f;\n      font-size: clamp(34px, 4vw, 54px);\n      line-height: 1.06;\n      letter-spacing: 0;\n      position: relative;\n      z-index: 2;\n    }\n\n    .aobo-hero p {\n      max-width: 940px;\n      margin: 0 0 12px;\n      font-size: 17px;\n      color: #314158;\n      position: relative;\n      z-index: 2;\n    }\n\n    .aobo-hero p:last-child {\n      margin-bottom: 0;\n    }\n\n    .aobo-article {\n      max-width: var(--aobo-page-width);\n      margin: 0 auto;\n    }\n\n    .aobo-article h2 {\n      margin: 44px 0 16px;\n      color: #082d6f;\n      font-size: 30px;\n      line-height: 1.25;\n      letter-spacing: 0;\n    }\n\n    .aobo-article h3 {\n      margin: 30px 0 10px;\n      color: #123f88;\n      font-size: 22px;\n      line-height: 1.3;\n      letter-spacing: 0;\n    }\n\n    .aobo-article p {\n      margin: 0 0 18px;\n      font-size: 17px;\n      color: var(--aobo-text);\n    }\n\n    .aobo-article a,\n    .aobo-hero a {\n      color: var(--aobo-blue);\n      font-weight: 700;\n      text-decoration: none;\n      transition: color 0.2s ease, background 0.2s ease;\n    }\n\n    .aobo-article a:hover,\n    .aobo-hero a:hover {\n      color: var(--aobo-orange);\n      background: var(--aobo-blue-soft);\n    }\n\n    .aobo-table-wrap {\n      overflow-x: auto;\n      margin: 22px 0 28px;\n      border-radius: 18px;\n      border: 1px solid var(--aobo-border);\n      box-shadow: 0 12px 32px rgba(12, 86, 208, 0.07);\n    }\n\n    .aobo-table {\n      width: 100%;\n      border-collapse: collapse;\n      background: var(--aobo-white);\n      min-width: 760px;\n    }\n\n    .aobo-table th {\n      background: var(--aobo-blue-soft);\n      color: #082d6f;\n      text-align: left;\n      padding: 14px 16px;\n      font-size: 15px;\n      vertical-align: top;\n    }\n\n    .aobo-table td {\n      padding: 14px 16px;\n      border-bottom: 1px solid #e8eef8;\n      vertical-align: top;\n      font-size: 15px;\n    }\n\n    .aobo-table tr:last-child td {\n      border-bottom: none;\n    }\n\n    .aobo-table td:first-child {\n      color: #082d6f;\n      font-weight: 700;\n    }\n\n    .aobo-note-box {\n      margin: 34px 0;\n      padding: 22px 24px;\n      border: 1px solid var(--aobo-border);\n      border-left: 5px solid var(--aobo-orange);\n      border-radius: 16px;\n      background: #fbfdff;\n      color: var(--aobo-muted);\n    }\n\n    .aobo-note-box p {\n      margin: 0 0 12px;\n      color: var(--aobo-muted);\n    }\n\n    .aobo-note-box p:last-child {\n      margin-bottom: 0;\n    }\n\n    .aobo-final-cta {\n      margin-top: 34px;\n      padding: 32px 34px;\n      border-radius: 24px;\n      background: linear-gradient(135deg, #073b91 0%, #0c56d0 100%);\n      color: #ffffff;\n      box-shadow: 0 18px 45px rgba(12, 86, 208, 0.20);\n      display: flex;\n      align-items: center;\n      justify-content: space-between;\n      gap: 20px;\n      flex-wrap: wrap;\n    }\n\n    .aobo-final-cta h2 {\n      margin: 0 0 12px;\n      color: #ffffff;\n      font-size: 26px;\n      line-height: 1.25;\n      letter-spacing: 0;\n    }\n\n    .aobo-final-cta p {\n      margin: 0;\n      color: rgba(255, 255, 255, 0.92);\n      max-width: 820px;\n      font-size: 16px;\n    }\n\n    .aobo-cta-buttons {\n      display: flex;\n      gap: 10px;\n      flex-wrap: wrap;\n      align-items: center;\n    }\n\n    .aobo-btn {\n      display: inline-flex;\n      align-items: center;\n      justify-content: center;\n      text-align: center;\n      min-height: 42px;\n      padding: 10px 18px;\n      border-radius: 999px;\n      text-decoration: none;\n      font-weight: 700;\n      font-size: 14px;\n      line-height: 1.2;\n      transition: all 0.2s ease;\n      cursor: pointer;\n      white-space: nowrap;\n    }\n\n    .aobo-final-cta .aobo-btn {\n      flex: 0 0 auto;\n      background: #ffffff;\n      border: 1px solid #ffffff;\n      color: var(--aobo-blue) !important;\n    }\n\n    .aobo-final-cta .aobo-btn:hover {\n      transform: translateY(-1px);\n      background: #fff7ed;\n      color: var(--aobo-blue-dark) !important;\n    }\n\n    .aobo-final-cta .aobo-btn-detail {\n      background: transparent;\n      border-color: rgba(255, 255, 255, 0.75);\n      color: #ffffff !important;\n    }\n\n    .aobo-final-cta .aobo-btn-detail:hover {\n      background: rgba(255, 255, 255, 0.14);\n      border-color: #ffffff;\n      color: #ffffff !important;\n    }\n\n    @media (max-width: 760px) {\n      .aobo-hero {\n        padding: 30px 22px;\n        border-radius: 22px;\n      }\n\n      .aobo-article h2 {\n        font-size: 25px;\n      }\n\n      .aobo-article h3 {\n        font-size: 20px;\n      }\n\n      .aobo-final-cta {\n        padding: 26px 22px;\n        border-radius: 22px;\n      }\n\n      .aobo-cta-buttons {\n        width: 100%;\n        flex-direction: column;\n        align-items: stretch;\n      }\n    }\n  <\/style>\n\n  <div class=\"aobo-wrap\">\n    <header class=\"aobo-hero\">\n      <span class=\"aobo-eyebrow\">D2 Tool Steel Machining Guide<\/span>\n      <h1>D2 Tool Steel Machining Parameters: Turning, Milling, Drilling &amp; Grinding<\/h1>\n      <p>D2 tool steel should normally be rough-machined in the annealed condition before heat treatment. In this condition, <a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel\/\">D2 tool steel<\/a> can be turned, milled, drilled, and ground with suitable carbide, cermet, or high-quality tool materials, but cutting speeds must be conservative because its chromium-rich carbides cause rapid tool wear.<\/p>\n      <p>After hardening to about 58&ndash;62 HRC, conventional turning, milling, and drilling become much more difficult. Hardened D2 is usually finished by grinding, EDM, PCBN hard turning, or controlled hard milling.<\/p>\n      <p>The correct parameters depend on the steel condition, tool material, machine rigidity, coolant control, and required surface finish.<\/p>\n    <\/header>\n\n    <main class=\"aobo-article\">\n      <h2>Quick Parameter Summary for D2 Tool Steel<\/h2>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead>\n            <tr><th>Operation<\/th><th>Material Condition<\/th><th>Recommended Tool or Process<\/th><th>Practical Note<\/th><\/tr>\n          <\/thead>\n          <tbody>\n            <tr><td>Rough turning<\/td><td>Annealed, about 200&ndash;250 HB<\/td><td>Coated carbide<\/td><td>Use conservative speed because D2 is abrasive<\/td><\/tr>\n            <tr><td>Finish turning<\/td><td>Annealed<\/td><td>Coated carbide or cermet<\/td><td>Cermet can run faster, but only with stable setup<\/td><\/tr>\n            <tr><td>Hard turning<\/td><td>Hardened, about 58&ndash;62 HRC<\/td><td>PCBN or ceramic<\/td><td>Mainly for finishing, not heavy stock removal<\/td><\/tr>\n            <tr><td>Milling<\/td><td>Annealed preferred<\/td><td>Coated carbide or high-quality HSS<\/td><td>Keep tool overhang short and avoid chatter<\/td><\/tr>\n            <tr><td>Hard milling<\/td><td>Hardened, about 58&ndash;62 HRC<\/td><td>Coated carbide or PCBN<\/td><td>Requires rigid machines and stable engagement<\/td><\/tr>\n            <tr><td>Drilling<\/td><td>Annealed preferred<\/td><td>Cobalt HSS, carbide-tipped, or solid carbide drills<\/td><td>Drill before hardening whenever possible<\/td><\/tr>\n            <tr><td>Grinding<\/td><td>Annealed or hardened<\/td><td>Conventional, SG, or CBN wheels<\/td><td>Control heat to avoid burn and cracks<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n\n      <h2>Factors That Influence D2 Machining Parameters<\/h2>\n      <p>D2 is difficult to machine because its high carbon and chromium content forms hard chromium-rich carbides in the steel matrix. These carbides give D2 strong wear resistance in service, but during machining they abrade the cutting edge and increase cutting forces.<\/p>\n      <p>A practical machinability rating for D2 is often around 45%, compared with 100% for a 1% carbon water-hardening tool steel such as W1. This means D2 normally requires lower cutting speeds, stronger cutting tools, rigid workholding, and careful heat control.<\/p>\n      <p>The steel condition has the biggest effect on parameter selection. Annealed D2 is much easier to machine because its spheroidized carbides are distributed in a softer matrix. Hardened D2, normally about 58&ndash;62 HRC in cold-work tooling, requires PCBN, ceramic tools, grinding, or EDM for final finishing.<\/p>\n      <p>For this reason, most stock removal should be completed before heat treatment. Post-hardening machining should be limited to final dimensional correction and surface finishing.<\/p>\n\n      <h2>Turning Parameters for Annealed D2 Tool Steel<\/h2>\n      <p>D2 is normally turned in the annealed condition before hardening. For parameter selection, annealed D2 is commonly treated as a 200&ndash;250 HB tool steel.<\/p>\n      <p>The following values are starting references, not fixed production standards. Actual parameters must be adjusted according to bar diameter, insert geometry, coating, machine rigidity, coolant condition, workholding stability, and surface finish requirements.<\/p>\n\n      <h3>Turning Parameters Using Coated Carbide Tools<\/h3>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead>\n            <tr><th>Operation<\/th><th>Depth of Cut<\/th><th>Feed Rate<\/th><th>Cutting Speed<\/th><th>Tool Grade<\/th><\/tr>\n          <\/thead>\n          <tbody>\n            <tr><td>Roughing<\/td><td>0.300 in.<\/td><td>0.015 ipr<\/td><td>200 sfm<\/td><td>C6 \/ M30, P30<\/td><\/tr>\n            <tr><td>Semiroughing<\/td><td>0.150 in.<\/td><td>0.010 ipr<\/td><td>275 sfm<\/td><td>C6 \/ M20, P20<\/td><\/tr>\n            <tr><td>Finishing<\/td><td>0.040 in.<\/td><td>0.005 ipr<\/td><td>575 sfm<\/td><td>C7 \/ M10, P10<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n      <p>Coated carbide tools are a practical choice for annealed D2 because they resist abrasive wear better than standard high-speed steel tools. If tool wear, chatter, or a poor surface finish occurs, reduce the cutting speed first, then check the rigidity of the setup before increasing the feed or depth of cut.<\/p>\n\n      <h3>Turning Parameters Using Cermet Tools<\/h3>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead>\n            <tr><th>Operation<\/th><th>Depth of Cut<\/th><th>Feed Rate<\/th><th>Cutting Speed<\/th><th>Tool Material<\/th><\/tr>\n          <\/thead>\n          <tbody>\n            <tr><td>Roughing<\/td><td>0.300 in.<\/td><td>0.015 ipr<\/td><td>550 sfm<\/td><td>HPC cermet<\/td><\/tr>\n            <tr><td>Semiroughing<\/td><td>0.150 in.<\/td><td>0.010 ipr<\/td><td>750 sfm<\/td><td>HPC cermet<\/td><\/tr>\n            <tr><td>Finishing<\/td><td>0.040 in.<\/td><td>0.005 ipr<\/td><td>1300 sfm<\/td><td>HPC cermet<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n      <p>Cermet tools can use higher cutting speeds than coated carbide tools, especially in semi-finish and finish turning. These higher speeds are only suitable when the machine, holder, and workpiece clamping are stable. If the setup is weak, coated carbide at a lower speed is usually safer.<\/p>\n\n      <h2>Hard Turning Parameters for Hardened D2 Tool Steel<\/h2>\n      <p>Hard turning may be used when D2 is hardened to 58&ndash;62 HRC, but it should be considered a finishing method. It is not a practical method for heavy stock removal.<\/p>\n      <p>PCBN tools are usually preferred for hardened D2 because they can resist high cutting temperatures and abrasive wear. Ceramic tools may also be used in suitable cases, but they require stable, continuous cutting and are less tolerant of interrupted cuts.<\/p>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead>\n            <tr><th>Condition<\/th><th>Tool Material<\/th><th>Cutting Speed<\/th><th>Feed Rate<\/th><th>Depth of Cut<\/th><th>Practical Use<\/th><\/tr>\n          <\/thead>\n          <tbody>\n            <tr><td>Hardened D2, about 58&ndash;62 HRC<\/td><td>PCBN<\/td><td>70&ndash;120 m\/min<\/td><td>0.08&ndash;0.20 mm\/rev<\/td><td>Light finishing cuts<\/td><td>Conservative starting range<\/td><\/tr>\n            <tr><td>Hardened D2, about 58 HRC<\/td><td>PCBN<\/td><td>80&ndash;120 m\/min<\/td><td>0.05&ndash;0.15 mm\/rev<\/td><td>About 0.2 mm<\/td><td>Surface finish optimization<\/td><\/tr>\n            <tr><td>Hardened steel baseline, 45&ndash;55 HRC<\/td><td>PCBN or ceramic<\/td><td>150&ndash;300 m\/min<\/td><td>0.15&ndash;0.20 mm\/rev<\/td><td>0.20&ndash;0.30 mm<\/td><td>General reference range<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n      <p>For hardened D2 at about 58 HRC, surface roughness values of about Ra 0.12&ndash;0.28 &micro;m can be achieved when speed, feed, depth of cut, tool geometry, and machine rigidity are properly controlled. For a better surface finish, use a lower feed rate and a stable cutting setup.<\/p>\n      <p>Hard turning is most suitable for cylindrical surfaces, stable geometries, and finishing cuts with good tool access. Grinding is still preferred when the part requires very tight flatness, sharp corners, extremely fine surface finish, or strict dimensional control.<\/p>\n      <p>For unsupported workpieces, keep the length-to-diameter ratio below 4:1 whenever possible to reduce chatter and deflection.<\/p>\n\n      <h2>Milling Guidelines for D2 Tool Steel<\/h2>\n      <p>D2 should be milled in the annealed condition whenever possible. Milling hardened D2 is possible, but it requires hard-milling tools, short tool projection, and a rigid machine.<\/p>\n\n      <h3>Milling Annealed D2 Tool Steel<\/h3>\n      <p>Annealed D2 is still abrasive, but it is much easier to mill than hardened D2. The main goal is to remove most of the stock before heat treatment, while leaving enough allowance for final finishing after hardening.<\/p>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead>\n            <tr><th>Milling Factor<\/th><th>Practical Recommendation<\/th><\/tr>\n          <\/thead>\n          <tbody>\n            <tr><td>Material condition<\/td><td>Mill in the annealed condition whenever possible<\/td><\/tr>\n            <tr><td>Tool material<\/td><td>Use coated carbide for better wear resistance; use high-quality HSS only for slower operations<\/td><\/tr>\n            <tr><td>Cutting speed<\/td><td>Use conservative speed because D2 carbides accelerate tool wear<\/td><\/tr>\n            <tr><td>Tool setup<\/td><td>Keep tool overhang short and use rigid holders<\/td><\/tr>\n            <tr><td>Workholding<\/td><td>Clamp the workpiece firmly and support the cutting area<\/td><\/tr>\n            <tr><td>Cutting strategy<\/td><td>Avoid unstable interrupted cuts and excessive radial engagement<\/td><\/tr>\n            <tr><td>Chip control<\/td><td>Maintain consistent chip evacuation with coolant, air blast, or tool supplier guidance<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n      <p>Carbide tools can run faster than HSS tools, but only when the machine, holder, and workpiece setup are rigid enough. If chatter occurs, lower the cutting speed, reduce radial engagement, and check tool projection.<\/p>\n\n      <h3>Hard Milling Hardened D2 Tool Steel<\/h3>\n      <p>Hard milling D2 at 58&ndash;62 HRC is mainly a finishing operation. It should not replace rough machining in the annealed condition.<\/p>\n      <p>Coated carbide tools may be used for hard milling when the setup is stable. PCBN end mills can produce finer finishes in suitable applications. In documented hard-milling trials, PCBN tools achieved surface roughness around Ra 0.1&ndash;0.2 &micro;m, while carbide ball-nose end mills produced rougher surfaces around Ra 1&ndash;2 &micro;m under difficult conditions.<\/p>\n      <p>For ball-end milling, tilting the tool by about 15&deg; to 20&deg; can move the cutting action away from the tool center, where the cutting speed is very low. This helps improve cutting stability and tool life.<\/p>\n\n      <h2>Drilling Guidelines for D2 Tool Steel<\/h2>\n      <p>D2 should be drilled before hardening whenever possible. Once hardened, conventional drilling becomes slow, expensive, and risky. For hardened D2, EDM or specialized carbide-drilling methods may be more practical.<\/p>\n      <p>D2 wears drills quickly because the drill margins and cutting lips continuously contact hard chromium carbides. This can cause margin wear, increased thrust, heat buildup, poor hole accuracy, and drill breakage.<\/p>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead>\n            <tr><th>Drilling Factor<\/th><th>Practical Recommendation<\/th><\/tr>\n          <\/thead>\n          <tbody>\n            <tr><td>Material condition<\/td><td>Drill in the annealed condition whenever possible<\/td><\/tr>\n            <tr><td>Tool material<\/td><td>Use cobalt HSS, carbide-tipped, or solid carbide drills depending on hole size and production volume<\/td><\/tr>\n            <tr><td>Coatings<\/td><td>TiN, TiCN, or TiAlN can improve wear resistance and reduce friction<\/td><\/tr>\n            <tr><td>Drill point<\/td><td>Use split-point geometry to reduce thrust and prevent walking<\/td><\/tr>\n            <tr><td>Point angle<\/td><td>118&deg; is common for annealed D2; 140&deg;&ndash;150&deg; may be used for harder conditions<\/td><\/tr>\n            <tr><td>Coolant<\/td><td>Use sufficient cutting fluid to control heat and flush chips<\/td><\/tr>\n            <tr><td>Deep holes<\/td><td>Use peck drilling or coolant-through drills<\/td><\/tr>\n            <tr><td>Hardened D2<\/td><td>Avoid standard drilling; consider EDM or special carbide drilling<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n      <p>For low-volume drilling in annealed D2, HSS drills may work, but tool wear will be faster than in simpler steels. For better hole accuracy and tool life, cobalt HSS, carbide-tipped, or solid carbide drills are preferred.<\/p>\n      <p>Deep holes need reliable chip evacuation. If chips pack in the flutes, coolant cannot reach the cutting edge, and the drill may fail quickly. Peck drilling or coolant-through drills help reduce this risk.<\/p>\n      <p>Avoid dwelling at the bottom of the hole. The drill must continue cutting at a stable feed rate. Rubbing without cutting generates heat and can damage the tool and workpiece surfaces.<\/p>\n\n      <h2>Grinding Parameters for D2 Tool Steel<\/h2>\n      <p>Grinding is commonly used after heat treatment to correct distortion, remove scale, and achieve the final tolerance. D2 is difficult to grind because its chromium carbides resist abrasive cutting. If grinding heat is not controlled, the surface may suffer from softening, rehardened layers, microcracks, or grinding cracks.<\/p>\n\n      <h3>Surface Grinding Parameters for D2 Tool Steel<\/h3>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead>\n            <tr><th>Condition \/ Hardness<\/th><th>Wheel Speed<\/th><th>Table Speed<\/th><th>Downfeed<\/th><th>Crossfeed<\/th><th>Wheel Identification<\/th><\/tr>\n          <\/thead>\n          <tbody>\n            <tr><td>Annealed, max 50 HRC<\/td><td>5500&ndash;6500 fpm<\/td><td>50&ndash;100 fpm<\/td><td>Rough: 0.003 in\/pass; finish: 0.0005 in\/pass max<\/td><td>0.050&ndash;0.500 in\/pass<\/td><td>A46JV<\/td><\/tr>\n            <tr><td>Hardened, 50&ndash;58 HRC<\/td><td>3000&ndash;4000 fpm<\/td><td>50&ndash;100 fpm<\/td><td>Rough: 0.002 in\/pass; finish: 0.0005 in\/pass max<\/td><td>0.025&ndash;0.250 in\/pass<\/td><td>A46IV<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n      <p>If CBN wheels are used for surface grinding annealed D2 up to about 50 HRC, wet wheel speeds may be increased to 5500&ndash;6000 fpm with a suitable CBN wheel such as B100T75B. For cylindrical grinding of annealed D2, an A60KV wheel may be used with wheel speeds of 5500&ndash;6500 fpm and work speeds of 60&ndash;100 fpm.<\/p>\n\n      <h3>Grinding Wheel and Coolant Selection<\/h3>\n      <p>For conventional grinding, use a wheel that cuts freely and does not glaze easily. A wheel that is too hard or too fine may rub instead of cut, causing excessive heat.<\/p>\n      <p>Advanced abrasives such as SG or vitrified CBN wheels may improve wheel life and thermal control in suitable applications. CBN wheels can be effective for hardened tool steels, but they still require correct coolant delivery, stable dressing, and controlled stock removal.<\/p>\n      <p>Coolant must continuously reach the grinding zone. Poor nozzle position, insufficient flow, or intermittent coolant can cause local overheating and thermal shock. If grinding burn, visible discoloration, surface softening, or microcracks are the main issues, this topic should be handled in a separate guide on preventing grinding burn in D2 tool steel.<\/p>\n\n      <h3>Post-Grinding Stress Relief<\/h3>\n      <p>For critical D2 tooling, a stress-relief temper after significant grinding is recommended. A practical post-grinding temper is usually performed below the original tempering temperature, typically by about 14&ndash;30&deg;C \/ 25&ndash;50&deg;F. This helps relieve residual stress and temper any freshly formed martensite without significantly reducing final hardness.<\/p>\n      <p>Grinding stability depends not only on parameters, but also on material quality. Aobo Steel supplies forged D2 tool steel with stable chemistry and ultrasonic inspection available for industrial tooling applications.<\/p>\n\n      <h2>Recommended Machining Sequence<\/h2>\n      <p>D2 machining parameters should be selected together with the manufacturing sequence. The best practice is to remove most material before hardening and reserve post-hardening operations for final finishing.<\/p>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead>\n            <tr><th>Stage<\/th><th>Recommended Operation<\/th><th>Purpose<\/th><\/tr>\n          <\/thead>\n          <tbody>\n            <tr><td>Raw material preparation<\/td><td>Remove scale, decarburized layer, and rough surface defects<\/td><td>Improve machining consistency<\/td><\/tr>\n            <tr><td>Rough machining<\/td><td>Machine in annealed condition<\/td><td>Remove most stock with lower tool wear<\/td><\/tr>\n            <tr><td>Stress relief<\/td><td>Apply after heavy rough machining when required<\/td><td>Reduce distortion during hardening<\/td><\/tr>\n            <tr><td>Semi-finish machining<\/td><td>Leave suitable allowance for heat-treatment movement<\/td><td>Prepare geometry before hardening<\/td><\/tr>\n            <tr><td>Heat treatment<\/td><td>Harden and temper to required working hardness<\/td><td>Achieve final wear resistance<\/td><\/tr>\n            <tr><td>Final finishing<\/td><td>Use grinding, EDM, PCBN hard turning, or hard milling<\/td><td>Achieve final tolerance and surface finish<\/td><\/tr>\n            <tr><td>Inspection<\/td><td>Check size, surface condition, and grinding damage<\/td><td>Reduce risk of premature tool failure<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n      <p>This sequence matters because hardened D2 is slow and costly to machine. If too much stock remains after heat treatment, grinding time increases, and the risk of burning or cracking rises.<\/p>\n\n      <h2>Practical Notes for Stable Machining D2 Steel<\/h2>\n      <p>Stable machining of D2 depends on the full machining system. Cutting speed and feed rate alone are not enough. The machine, toolholder, fixture, workpiece support, coolant delivery, and tool material must be matched to the operation.<\/p>\n      <p>Rigidity is the first requirement. Keep the tool overhang short, clamp the workpiece close to the cutting area, and avoid weak setups. For unsupported turning or boring, keeping the length-to-diameter ratio below 4:1 helps reduce deflection and chatter.<\/p>\n      <p>Chatter must be controlled early. If vibration appears, carbide and ceramic tools can chip quickly. In milling, reduce unstable engagement and check cutter pitch, radial depth of cut, and tool projection. When turning, check the holder&#8217;s rigidity, nose radius, and edge preparation.<\/p>\n      <p>Coolant strategy must be consistent. In conventional machining, stable coolant flow helps remove heat and chips. In hard milling, flood coolant may cause thermal shock in some cases, so air blast or minimum-quantity lubrication may be preferred depending on the tool supplier&#8217;s guidance. Intermittent coolant should be avoided.<\/p>\n      <p>Tool material should match the D2 condition. Coated carbide is suitable for turning and milling annealed D2. Cermet may be used for higher-speed finishing when the setup is stable. PCBN and ceramic tools are suitable for finishing hardened D2. Standard uncoated HSS tools should be used carefully because D2 can wear them rapidly.<\/p>\n      <p>For drilling, power feed is preferred over hand feeding. A constant feed helps the drill cut rather than rub. Hole entrances and exits should be deburred or lightly chamfered to reduce stress concentration in tooling components.<\/p>\n    <\/main>\n\n    <section class=\"aobo-final-cta\">\n      <div>\n        <h2>Need D2 Tool Steel for Machining and Heat Treatment Preparation?<\/h2>\n        <p>We supply D2 tool steel in annealed condition, suitable for rough machining before heat treatment. For bulk orders, we can provide round bars and plates with machining allowance, stable chemistry, and inspection support.<\/p>\n      <\/div>\n      <div class=\"aobo-cta-buttons\">\n        <a class=\"aobo-btn aobo-btn-detail\" href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel\/\">View D2 Tool Steel<\/a>\n        <a class=\"aobo-btn hs-cta-trigger-button hs-cta-trigger-button-230288465624\" href=\"javascript:void(0);\">Send Inquiry<\/a>\n      <\/div>\n    <\/section>\n  <\/div>\n<\/section>","protected":false},"excerpt":{"rendered":"<p>D2 Tool Steel Machining Guide D2 Tool Steel Machining Parameters: Turning, Milling, Drilling &amp; Grinding D2 tool steel should normally be rough-machined in the annealed condition before heat treatment. In this condition, D2 tool steel can be turned, milled, drilled, and ground with suitable carbide, cermet, or high-quality tool materials, but cutting speeds must be [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":15063,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"content-type":"","_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"disabled","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-13401","page","type-page","status-publish","has-post-thumbnail","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v27.7 (Yoast SEO v27.7) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding<\/title>\n<meta name=\"description\" content=\"Find practical D2 tool steel machining parameters for turning, milling, drilling, hard turning, and grinding. Aobo Steel explains how to machine annealed and hardened D2.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel-machining-parameters\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding\" \/>\n<meta property=\"og:description\" content=\"Find practical D2 tool steel machining parameters for turning, milling, drilling, hard turning, and grinding. Aobo Steel explains how to machine annealed and hardened D2.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel-machining-parameters\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-06-04T00:43:04+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif\" \/>\n\t<meta property=\"og:image:width\" content=\"1254\" \/>\n\t<meta property=\"og:image:height\" content=\"1254\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"11\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding\",\"datePublished\":\"2026-03-10T03:09:23+00:00\",\"dateModified\":\"2026-06-04T00:43:04+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/\"},\"wordCount\":2298,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif\",\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/\",\"name\":\"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif\",\"datePublished\":\"2026-03-10T03:09:23+00:00\",\"dateModified\":\"2026-06-04T00:43:04+00:00\",\"description\":\"Find practical D2 tool steel machining parameters for turning, milling, drilling, hard turning, and grinding. Aobo Steel explains how to machine annealed and hardened D2.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif\",\"width\":1254,\"height\":1254},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-tool-steel-machining-parameters\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding","description":"Find practical D2 tool steel machining parameters for turning, milling, drilling, hard turning, and grinding. Aobo Steel explains how to machine annealed and hardened D2.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/d2-tool-steel-machining-parameters\/","og_locale":"ko_KR","og_type":"article","og_title":"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding","og_description":"Find practical D2 tool steel machining parameters for turning, milling, drilling, hard turning, and grinding. Aobo Steel explains how to machine annealed and hardened D2.","og_url":"https:\/\/aobosteel.com\/ko\/d2-tool-steel-machining-parameters\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-06-04T00:43:04+00:00","og_image":[{"width":1254,"height":1254,"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif","type":"image\/png"}],"twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"11\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding","datePublished":"2026-03-10T03:09:23+00:00","dateModified":"2026-06-04T00:43:04+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/"},"wordCount":2298,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif","inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/","url":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/","name":"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif","datePublished":"2026-03-10T03:09:23+00:00","dateModified":"2026-06-04T00:43:04+00:00","description":"Find practical D2 tool steel machining parameters for turning, milling, drilling, hard turning, and grinding. Aobo Steel explains how to machine annealed and hardened D2.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/"]}]},{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif","width":1254,"height":1254},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/d2-tool-steel-machining-parameters\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"D2 Tool Steel Machining Parameters: Speeds, Feeds &amp; Grinding"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif",1254,1254,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-150x150.avif",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-300x300.avif",300,300,true],"medium_large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-768x768.avif",768,768,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-1024x1024.avif",1024,1024,true],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif",1254,1254,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif",1254,1254,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-12x12.avif",12,12,true]},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"D2 Tool Steel Machining Guide D2 Tool Steel Machining Parameters: Turning, Milling, Drilling &amp; Grinding D2 tool steel should normally be rough-machined in the annealed condition before heat treatment. In this condition, D2 tool steel can be turned, milled, drilled, and ground with suitable carbide, cermet, or high-quality tool materials, but cutting speeds must be&hellip;","rttpg_featured_image_url":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif",1254,1254,false],"landscape":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif",1254,1254,false],"portraits":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif",1254,1254,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-150x150.avif",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-300x300.avif",300,300,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-1024x1024.avif",1024,1024,true],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif",1254,1254,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad.avif",1254,1254,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/Recommended-Cutting-Parameters-for-D2-Tool-Steel-ad-12x12.avif",12,12,true]},"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"D2 Tool Steel Machining Guide D2 Tool Steel Machining Parameters: Turning, Milling, Drilling &amp; Grinding D2 tool steel should normally be rough-machined in the annealed condition before heat treatment. In this condition, D2 tool steel can be turned, milled, drilled, and ground with suitable carbide, cermet, or high-quality tool materials, but cutting speeds must be&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/13401","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=13401"}],"version-history":[{"count":0,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/13401\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media\/15063"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=13401"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}