{"id":13242,"date":"2026-03-04T08:33:30","date_gmt":"2026-03-04T00:33:30","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=13242"},"modified":"2026-10-16T12:25:33","modified_gmt":"2026-10-16T04:25:33","slug":"d2-vs-a2-tool-steel","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/d2-vs-a2-tool-steel\/","title":{"rendered":"D2 \uacf5\uad6c\uac15\uacfc A2 \uacf5\uad6c\uac15 \ube44\uad50: \ub9c8\ubaa8, \uce69\ud551 \ubc0f \uc120\ud0dd \uac00\uc774\ub4dc"},"content":{"rendered":"<h1 class=\"wp-block-heading\">D2 \uacf5\uad6c\uac15\uacfc A2 \uacf5\uad6c\uac15: \uc2e4\uc6a9\uc801\uc778 \uc120\ud0dd \uac00\uc774\ub4dc<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"https:\/\/aobosteel.com\/ko\/d2-steel-properties\/\">D2 \uacf5\uad6c\uac15<\/a> \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel-properties\/\">A2 \uacf5\uad6c\uac15<\/a> \ub458 \ub2e4 \uacf5\uae30 \uacbd\ud654\ud615 \ub0c9\uac04 \uac00\uacf5 \uacf5\uad6c\uac15\uc774\uc9c0\ub9cc, \uc11c\ub85c \ub2e4\ub978 \uacf5\uad6c \ubb38\uc81c\ub97c \ud574\uacb0\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub0b4\ub9c8\ubaa8\uc131, \ub0a0 \uc720\uc9c0\ub825, \uae34 \uc218\uba85\uc774 \uac00\uc7a5 \uc911\uc694\ud55c \uacbd\uc6b0\uc5d0\ub294 D2\uac15\uc774 \ub354 \ub098\uc740 \uc120\ud0dd\uc785\ub2c8\ub2e4. \ub0b4\ud30c\uc190\uc131, \ub0b4\uade0\uc5f4\uc131, \uac00\uacf5 \uc6a9\uc774\uc131, \uc81c\uc791 \ub09c\uc774\ub3c4\uac00 \ub354 \uc911\uc694\ud55c \uacbd\uc6b0\uc5d0\ub294 A2\uac15\uc774 \ub354 \ub098\uc740 \uc120\ud0dd\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucc28\uc774\ub294 \uc8fc\ub85c \ub2e4\uc74c\uc5d0\uc11c \ube44\ub86f\ub429\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-carbide-types-and-hardness\/\">\ucd08\uacbd \ud569\uae08 \ubd80\ud53c<\/a>. D2\ub294 \ud0c4\uc18c\uc640 \ud06c\ub86c \ud568\ub7c9\uc774 \ub354 \ub192\uc544 \ub354 \ub2e8\ub2e8\ud55c \ud0c4\ud654\ubb3c\uc744 \ud615\uc131\ud558\uc5ec \ub0b4\ub9c8\ubaa8\uc131\uc774 \ud5a5\uc0c1\ub429\ub2c8\ub2e4. A2\ub294 \ud070 \ud0c4\ud654\ubb3c\uc774 \uc801\uc5b4 \uc778\uc131\uc774 \ub354 \uc6b0\uc218\ud558\uace0 \uac00\uacf5\uc774 \ub354 \uc27d\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ube60\ub978 \uc120\ud0dd \ud14c\uc774\ube14<\/h2>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uacf5\uad6c \uc694\uad6c \uc0ac\ud56d<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub098\uc740 \uc120\ud0dd<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc65c<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub0b4\ub9c8\ubaa8\uc131<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud0c4\ud654\ubb3c \ud568\ub7c9\uc774 \ub354 \ub192\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5e3\uc9c0 \uc720\uc9c0<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubaa8\uc11c\ub9ac \ub465\uae00\ub9bc\uc5d0 \ub300\ud55c \uc800\ud56d\ub825\uc774 \ub354 \ub6f0\uc5b4\ub0a9\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc7a5\uae30 \uc0dd\uc0b0<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0a0\uce74\ub86d\uac8c \uac08\uc544\uc57c \ud558\ub294 \uc8fc\uae30\uac00 \ub354 \uae38\uc5b4\uc9d1\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uce69\ud551 \uc800\ud56d\uc131<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubaa8\uc11c\ub9ac \uc778\uc131\uc774 \ud5a5\uc0c1\ub418\uc5c8\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uade0\uc5f4 \uc800\ud56d\uc131<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0a0\uce74\ub85c\uc6b4 \ubaa8\uc11c\ub9ac\uc640 \uc751\ub825 \uc9d1\uc911 \ud604\uc0c1\uc5d0 \ub35c \ubbfc\uac10\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \uc815\ub3c4\uc758 \ucda9\uaca9 \ud558\uc911<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubd80\ud558\uac00 \uac04\ud5d0\uc801\uc73c\ub85c \ubc1c\uc0dd\ud560 \uacbd\uc6b0 D2\ubcf4\ub2e4 \uc548\uc804\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \uc26c\uc6b4 \uac00\uacf5<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc808\uc0ad \uc911 \ud0c4\ud654\ubb3c \uac04\uc12d\uc774 \uc801\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \uc27d\uac8c \uac08 \uc218 \uc788\uc2b5\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc0ad \ub09c\uc774\ub3c4 \ubc0f \ud45c\uba74 \uc190\uc0c1 \uc704\ud5d8\uc774 \ub0ae\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc81c\uc870 \ube44\uc6a9 \uc808\uac10<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uac00\uacf5 \ubc0f \ub9c8\ubb34\ub9ac \uc2dc\uac04 \ub2e8\ucd95.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub9c8\ubaa8\uc131 \ud658\uacbd\uc5d0\uc11c \ucd5c\ub300 \ub9c8\ubaa8 \uc218\uba85<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc7a5\uae30\uc801\uc778 \ub9c8\ubaa8 \uc131\ub2a5\uc774 \ub354 \uc6b0\uc218\ud569\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">\ud654\ud559 \uc870\uc131 \ube44\uad50<\/h2>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc694\uc18c<\/th><th class=\"has-text-align-left\" data-align=\"left\">D2 \uacf5\uad6c\uac15<\/th><th class=\"has-text-align-left\" data-align=\"left\">A2 \uacf5\uad6c\uac15<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud0c4\uc18c<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.40% ~ 1.60%<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.95%\uc5d0\uc11c 1.05%\uae4c\uc9c0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.00% ~ 13.50%<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.75% ~ 5.50%<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubab0\ub9ac\ube0c\ub374<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70%\uc5d0\uc11c 1.20%\uae4c\uc9c0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.90%\uc5d0\uc11c 1.40%\uae4c\uc9c0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubc14\ub098\ub4d0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.50% ~ 1.10%<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15% ~ 0.50%<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Manganese<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20% ~ 0.60%<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.40% ~ 1.00%<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Silicon<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.10% ~ 0.60%<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.10% ~ 0.60%<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">D2 \ubc0f A2 \uacf5\uad6c\uac15\uc758 \ub3d9\ub4f1 \ub4f1\uae09<\/h2>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud45c\uc900\/\uc9c0\uc5ed<\/th><th class=\"has-text-align-left\" data-align=\"left\">D2 \uacf5\uad6c\uac15<\/th><th class=\"has-text-align-left\" data-align=\"left\">A2 \uacf5\uad6c\uac15<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">AISI \/ ASTM<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">UNS<\/td><td class=\"has-text-align-left\" data-align=\"left\">T30402<\/td><td class=\"has-text-align-left\" data-align=\"left\">T30102<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc601\uc5b4\/ISO<\/td><td class=\"has-text-align-left\" data-align=\"left\">X153CrMoV12 \/ X160CrMoV12-1<\/td><td class=\"has-text-align-left\" data-align=\"left\">X100CrMoV5 \/ X100CrMoV5-1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">DIN \/ W-Nr.<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.2379<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.2363<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">JIS<\/td><td class=\"has-text-align-left\" data-align=\"left\">SKD11<\/td><td class=\"has-text-align-left\" data-align=\"left\">SKD12<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">BS<\/td><td class=\"has-text-align-left\" data-align=\"left\">BD2<\/td><td class=\"has-text-align-left\" data-align=\"left\">BA2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AFNOR<\/td><td class=\"has-text-align-left\" data-align=\"left\">Z160CDV12 \/ X160CrMoV12<\/td><td class=\"has-text-align-left\" data-align=\"left\">Z100CDV5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">GB<\/td><td class=\"has-text-align-left\" data-align=\"left\">Cr12Mo1V1<\/td><td class=\"has-text-align-left\" data-align=\"left\">Cr5Mo1V<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">SS \uc2a4\uc6e8\ub374<\/td><td class=\"has-text-align-left\" data-align=\"left\">2310<\/td><td class=\"has-text-align-left\" data-align=\"left\">2260<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">UNI \uc774\ud0c8\ub9ac\uc544<\/td><td class=\"has-text-align-left\" data-align=\"left\">X155CrVMo12-1KU \ub610\ub294 \uc774\uc640 \uc720\uc0ac\ud55c \ud45c\uae30 \ubcc0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">X100CrMoV5-1KU<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">D2\ub294 \uc77c\ubc18\uc801\uc73c\ub85c \ub2e4\uc74c \ub4f1\uae09\uacfc \ub300\uc751\ub429\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel-1-2379-skd11-selection-supply-guide\/\">1.2379 \/ X153CrMoV12 \/ SKD11<\/a>. A2\ub294 \uc77c\ubc18\uc801\uc73c\ub85c 1.2363 \/ X100CrMoV5 \/ SKD12\uc640 \ub300\uc751\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub4f1\uac00 \ub4f1\uae09\uc740 \uc18c\uc2f1 \ubc0f \uacac\uc801\uc5d0 \uc720\uc6a9\ud558\uc9c0\ub9cc, \uc0ac\uc6a9\uc790\ub294 \uc5ec\uc804\ud788 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-quality-verification\/\">\uc815\ud655\ud55c \ud45c\uc900\uc744 \ud655\uc778\ud574\uc57c \ud569\ub2c8\ub2e4<\/a>, \ud654\ud559 \uc870\uc131, \ub0a9\ud488 \uc0c1\ud0dc \ubc0f \uc5f4\ucc98\ub9ac \uc694\uad6c \uc0ac\ud56d\uc744 \ud655\uc778\ud574\uc57c \ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uacbd\ub3c4 \ubc0f \uc5f4\ucc98\ub9ac<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">D2\uc640 A2\ub294 \uc5f4\ucc98\ub9ac \ud6c4 <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel-hardness\/\">\uc720\uc0ac\ud55c \uc0ac\uc6a9 \uacbd\ub3c4<\/a> \ub97c \ub2ec\uc131\ud560 \uc218 \uc788\uc73c\ubbc0\ub85c, HRC\ub9cc\uc73c\ub85c \uc131\ub2a5\uc744 \ud310\ub2e8\ud574\uc11c\ub294 \uc548 \ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc694\uc778<\/th><th class=\"has-text-align-left\" data-align=\"left\">D2 \uacf5\uad6c\uac15<\/th><th class=\"has-text-align-left\" data-align=\"left\">A2 \uacf5\uad6c\uac15<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \uc0c1\ud0dc \uacbd\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 61~65 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 62~65 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc77c\ubc18 \uc0ac\uc6a9 \uacbd\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4 58~60 HRC \uc815\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4 58~60 HRC \uc815\ub3c4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub192\uc740 \ub9c8\ubaa8 \ubc94\uc704<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 60~62 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc77c\ubd80 \uc751\uc6a9 \ubd84\uc57c\uc5d0\uc11c \uac00\ub2a5\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub0b4\uad6c\uc131\uc5d0 \uc911\uc810\uc744 \ub454 \uc81c\ud488\uad70<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 56~58 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 56~58 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc77c\ubc18\uc801\uc73c\ub85c \ud654\uc528 1850\ub3c4 \/ \uc12d\uc528 1010\ub3c4 \uc815\ub3c4\uc785\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc77c\ubc18\uc801\uc73c\ub85c \ud654\uc528 1775\ub3c4 \/ \uc12d\uc528 968\ub3c4 \uc815\ub3c4\uc785\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uc794\ub958\ubb3c \ubb38\uc81c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub192\uc740<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0ae\ucd94\ub2e4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc0ad \uac10\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub192\uc740<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0ae\ucd94\ub2e4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uce58\uc218 \uc548\uc815\uc131<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc81c\ub300\ub85c \uc81c\uc5b4\ud558\uba74 \ud6cc\ub96d\ud55c \uc131\ub2a5\uc744 \ubc1c\ud718\ud569\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud6cc\ub96d\ud558\uace0 \ub300\uccb4\ub85c \uc608\uce21 \uac00\ub2a5\ud569\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">D2\ub294 \ud569\uae08 \ud568\ub7c9\uc774 \ub192\uace0 \ub2e4\uc74c\uc758 \uc704\ud5d8 \ub54c\ubb38\uc5d0 \ub2f4\uae08\uc9c8, \ub728\uc784 \ubc0f \uc5f0\uc0ad \uc911 \ub354 \uc5c4\uaca9\ud55c \uad00\ub9ac\uac00 \ud544\uc694\ud569\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/d2-austenitizing-temperature\/\">\uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A2\ub294 \uc77c\ubc18\uc801\uc73c\ub85c <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel-heat-treatment-guide\/\">\uc5f4\ucc98\ub9ac\uc5d0\uc11c \ub354 \uad00\ub300\ud569\ub2c8\ub2e4<\/a> \ubc0f \ub9c8\ubb34\ub9ac \uac00\uacf5\uc5d0\uc11c \ub354 \uad00\ub300\ud569\ub2c8\ub2e4. \uc774\ub294 \ub354 \ubcf5\uc7a1\ud55c \ud615\uc0c1\uc774\ub098 \ub354 \uc5c4\uaca9\ud55c \uc81c\uc870 \uad00\ub9ac \uc694\uad6c \uc0ac\ud56d\uc774 \uc788\ub294 \uacf5\uad6c\uc5d0 \uc790\uc8fc \uc0ac\uc6a9\ub418\ub294 \uc774\uc720 \uc911 \ud558\ub098\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uac00\uacf5\uc131, \uc5f0\uc0ad \ubc0f \uc81c\uc791 \ube44\uc6a9<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A2\ub294 <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel-machining-fabrication-guide\/\">\uc644\uc131\ub41c \uacf5\uad6c\ub85c \uc81c\uc870\ud558\uae30 \ub354 \uc27d\uc2b5\ub2c8\ub2e4<\/a> . \uc774\ub294 \uacf5\uad6c\uc5d0 \ubcf5\uc7a1\ud55c \ud504\ub85c\ud30c\uc77c, \ub0a0\uce74\ub85c\uc6b4 \ub0b4\ubd80 \ucf54\ub108, \uc587\uc740 \ub2e8\uba74 \ub610\ub294 \ube48\ubc88\ud55c \uc7ac\uc5f0\uc0ad \uc694\uad6c \uc0ac\ud56d\uc774 \uc788\uc744 \ub54c \uc911\uc694\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ucc98\ub9ac \uc694\uc18c<\/th><th class=\"has-text-align-left\" data-align=\"left\">D2 \uacf5\uad6c\uac15<\/th><th class=\"has-text-align-left\" data-align=\"left\">A2 \uacf5\uad6c\uac15<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1 \ucc98\ub9ac \uc0c1\ud0dc\uc5d0\uc11c\uc758 \uac00\uacf5\uc131<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0ae\ucd94\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub098\uc740<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc77c\ubc18\uc801\uc778 \uac00\uacf5\uc131 \ub4f1\uae09<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 45%<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 60%<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc808\uc0ad \uacf5\uad6c \ub9c8\ubaa8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub192\uc740<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0ae\ucd94\ub2e4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc0ad \ub09c\uc774\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub192\uc740<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubcf4\ud1b5\uc758<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc7ac\uc5f0\ub9c8 \ube44\uc6a9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub192\uc740<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0ae\ucd94\ub2e4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\uc0ad \ud654\uc0c1 \ub610\ub294 \uade0\uc5f4 \ubc1c\uc0dd \uc704\ud5d8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub192\uc740<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub0ae\uc544\uc9c0\uc9c0\ub9cc \uc5ec\uc804\ud788 \uc81c\uc5b4\uac00 \ud544\uc694\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ucd5c\uc801\uc758 \uacbd\uc81c\uc801 \ud65c\uc6a9<\/td><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/abrasive-wear-resistant-tool-steels\/\">\uc7a5\uae30 \uc5f0\ub9c8\uc7ac \uc0dd\uc0b0<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/how-to-select-tool-steels\/\">\ub2e8\uae30 \ub610\ub294 \uc911\uae30 \uc0dd\uc0b0\uc6a9 \uacf5\uad6c \ub610\ub294 \ubcf5\uc7a1\ud55c \uacf5\uad6c<\/a><\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">D2\ub294 \ub9c8\ubaa8\uac00 \uac00\ub3d9 \uc911\ub2e8\uc758 \uc8fc\uc694 \uc6d0\uc778\uc77c \uacbd\uc6b0 \ub354 \ub192\uc740 \ucc98\ub9ac \ube44\uc6a9\uc744 \uc815\ub2f9\ud654\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uacf5\uad6c\uc5d0 D2 \uc218\uc900\uc758 \ub0b4\ub9c8\ubaa8\uc131\uc774 \ud544\uc694\ud558\uc9c0 \uc54a\uc740 \uacbd\uc6b0, \ud2b9\ud788 \ub2e8\uae30 \ub610\ub294 \uc911\uae30 \uc0dd\uc0b0\uc758 \uacbd\uc6b0 A2 \uac15\uc7ac\uac00 \ub354 \uacbd\uc81c\uc801\uc778 \uacbd\uc6b0\uac00 \ub9ce\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uace0\uc7a5 \ubaa8\ub4dc\uc5d0 \ub530\ub978 \uc120\ud0dd<\/h2>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uace0\uc7a5 \ubaa8\ub4dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc678\uad00<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub098\uc740 \uc120\ud0dd<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc2e4\uc6a9\uc801\uc778 \ucc38\uace0 \uc0ac\ud56d<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\ub9c8 \ub9c8\ubaa8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud45c\uba74 \ub9c8\ubaa8, \ubaa8\uc11c\ub9ac \ubb34\ub38c\uc9d0, \uacf5\ucc28 \uc190\uc2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2\ub97c \uc120\ud0dd\ud574\uc57c \ud558\ub294 \uac00\uc7a5 \uac15\ub825\ud55c \uc774\uc720<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubaa8\uc11c\ub9ac \ub465\uae00\uac8c \ucc98\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc808\uc0ad\ub0a0\uc740 \uc810\ucc28 \ub0a0\uce74\ub85c\uc6c0\uc744 \uc783\ub294\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2\ub294 \ub354 \uc624\ub7ab\ub3d9\uc548 \ub0a0\uce74\ub85c\uc6b4 \ubaa8\uc11c\ub9ac\ub97c \uc720\uc9c0\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc7a6\uc740 \uc7ac\ubd84\uc1c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacf5\uad6c\uac00 \ub108\ubb34 \ube68\ub9ac \ub9c8\ubaa8\ub429\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub9c8\ubaa8\uac00 \uc2ec\ud55c \uc7a5\uc2dc\uac04 \uc791\uc5c5\uc5d0 \uc720\uc6a9\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uce58\ud551<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uac00\uc7a5\uc790\ub9ac\uc5d0\uc11c \uc791\uc740 \uc870\uac01\ub4e4\uc774 \ub5a8\uc5b4\uc838 \ub098\uc635\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2\ub294 \ub108\ubb34 \uc798 \ubd80\uc11c\uc9c8 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ubd84\ud574<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacf5\uad6c\uac00 \ubaa8\uc11c\ub9ac, \uad6c\uba4d \ub610\ub294 \uc587\uc740 \ubd80\ubd84\uc5d0\uc11c \ud30c\uc190\ub429\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud615\uc0c1 \ubc0f \uc751\ub825 \uc9d1\uc911\uc744 \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc911\uac04 \uc815\ub3c4\uc758 \ucda9\uaca9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc911\ub2e8\ub41c \ub85c\ub529 \ub610\ub294 \ubaa8\uc11c\ub9ac \ucda9\uaca9<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc2ec\uac01\ud55c \ucda9\uaca9\uc5d0\ub294 S \uc2dc\ub9ac\uc988 \uac15\ucca0\uc774 \ud544\uc694\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubd84\uc1c4 \ud53c\ud574<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc644\uc131 \ud6c4 \uade0\uc5f4\uc774\ub098 \uadf8\uc744\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2\ub294 \uc548\uc804\ud558\uac8c \uc5f0\ub9c8\ud558\uae30\uac00 \ub354 \uc27d\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc18c\uc131 \ubcc0\ud615<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacf5\uad6c\uac00 \ud718\uac70\ub098, \ubc84\uc12f\ucc98\ub7fc \ubd80\ud480\uc5b4 \uc624\ub974\uac70\ub098, \ubaa8\uc591\uc774 \ubcc0\ud615\ub429\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uba3c\uc800 \uacbd\ub3c4\ub97c \ud655\uc778\ud558\uc138\uc694<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubb38\uc81c\ub294 \uc5f4\ucc98\ub9ac \ub610\ub294 \uacf5\uad6c \uc9c0\uc9c0\ub825\uc5d0 \uc788\uc744 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\uc18c\uc131 \ubcc0\ud615\uc758 \uacbd\uc6b0 A2\uc5d0\uc11c D2\ub85c \ubcc0\uacbd\ud558\ub294 \uac83\uc774 \ud56d\uc0c1 \ub2f5\uc740 \uc544\ub2d9\ub2c8\ub2e4. \uba3c\uc800 <a href=\"https:\/\/aobosteel.com\/ko\/hardness-testing-methods\/\">\uacbd\ub3c4\ub97c \ud655\uc778\ud558\uc2ed\uc2dc\uc624<\/a>, \uc5f4\ucc98\ub9ac, \ud558\uc911 \uc9c0\uc9c0, \ub2e8\uba74 \ud06c\uae30 \ubc0f \uacf5\uad6c \uc124\uacc4\ub97c \ud655\uc778\ud558\uc2ed\uc2dc\uc624. \uc7ac\ub8cc\ub97c \ubcc0\uacbd\ud558\uae30 \uc804\uc5d0 \ud30c\uc190\uc774 \uacfc\ubd80\ud558, \ubd80\uc801\uc808\ud55c \uae08\ud615 \ud074\ub9ac\uc5b4\ub7f0\uc2a4 \ub610\ub294 \ubd88\ucda9\ubd84\ud55c \uc9c0\uc9c0 \ub54c\ubb38\uc778\uc9c0 \uace0\ub824\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub2e4\uc74c\uc73c\ub85c \uc778\ud574 \ud30c\uc190\ub418\ub294 \uacf5\uad6c\uc758 \uacbd\uc6b0 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steels-for-chipping-resistance\/\">\uce69\ud551<\/a>, \ub0a0 \ud615\uc0c1, \ud45c\uba74 \ub9c8\uac10 \ubc0f \ucda9\uaca9 \ud558\uc911\uc744 \uac80\ud1a0\ud558\uc2ed\uc2dc\uc624. \ub2e4\uc74c\uc744 \ubcf4\uc774\ub294 \uacf5\uad6c\uc758 \uacbd\uc6b0 <a href=\"https:\/\/aobosteel.com\/ko\/tool-and-die-failure-analysis\/\">\uae09\uc18d \ub9c8\ubaa8<\/a>, \uac15\uc7ac \uc120\ud0dd\ubfd0\ub9cc \uc544\ub2c8\ub77c \uc724\ud65c \ubc0f \uc815\ub82c \uc870\uac74\uc744 \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">D2 \ub610\ub294 A2\uac00 \uc801\uc808\ud55c \uc120\ud0dd\uc774 \uc544\ub2d0 \ub54c<\/h2>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\ud669<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud53c\ud558\ub2e4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub098\uc740 \ubc29\ud5a5<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc2ec\ud55c \ucda9\uaca9 \ub610\ub294 \uad6c\ud0c0<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2 \ubc0f \ub54c\ub54c\ub85c A2<\/td><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/s7-tool-steel\/\">S7<\/a> \ub610\ub294 \uae30\ud0c0 \ucda9\uaca9 \ubc29\uc9c0 \uacf5\uad6c\uac15<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc9c4\uc815\ud55c \uc5f4 \uc791\uc5c5 \uc11c\ube44\uc2a4<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2\uc640 A2<\/td><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel\/\">H13<\/a>, <a href=\"https:\/\/aobosteel.com\/ko\/h11-tool-steel\/\">H11<\/a>, \ub610\ub294 \uae30\ud0c0 <a href=\"https:\/\/aobosteel.com\/ko\/hot-work-tool-steels\/\">\uace0\uc628 \uc791\uc5c5\uc6a9 \uacf5\uad6c\uac15<\/a><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uace0\uc18d \uc808\uc0ad<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2\uc640 A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\uc18d\uac15<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \ub9c8\ubaa8 \uc694\uad6c\ub7c9<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2 \uc774\uc0c1\uc758 \ub0b4\ub9c8\ubaa8\uc131 \ub0c9\uac04 \uac00\uacf5 \ub4f1\uae09<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud30c\uc190 \uc774\ub825\uc774 \uc788\ub294 \ubcf5\uc7a1\ud55c \uacf5\uad6c<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2 \ub610\ub294 \uadf8\ubcf4\ub2e4 \ub354 \ub192\uc740 \ub4f1\uae09<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc7a6\uc740 \uc6a9\uc811 \uc218\ub9ac\uac00 \uc608\uc0c1\ub429\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc6a9\uc811\uc131\uc774 \ub354 \uc88b\uc740 \uac15\uc7ac \uc0ac\uc6a9 \ub610\ub294 \uacf5\uad6c \uc7ac\uc124\uacc4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uac70\uc6b8\ucc98\ub7fc \uad11\ud0dd\uc744 \ub0b4\uc57c \ud569\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud0c4\ud654\ubb3c \ud568\ub7c9\uc774 \ub0ae\uc740 \uac15\ucca0\uc77c\uc218\ub85d \uc5f0\ub9c8 \uc131\ub2a5\uc774 \ub354 \uc88b\uc744 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc800\ubd80\ud558 \ub2e8\uc21c \ubd80\ud488<\/td><td class=\"has-text-align-left\" data-align=\"left\">D2 \ub610\ub294 A2\uac00 \uacfc\ub3c4\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/ko\/o1-tool-steel\/\">O1<\/a>, 4140 \ub610\ub294 \uc800\ub834\ud55c \uac15\ucca0\ub85c\ub3c4 \ucda9\ubd84\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">\ub9c8\ubaa8\uac00 \uc8fc\ub41c \uacf5\uad6c\uc5d0\ub294 D2\ub97c \uc120\ud0dd\ud558\uc2ed\uc2dc\uc624.<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\ub0b4\ub9c8\ubaa8\uc131, \ub0a0 \uc720\uc9c0\ub825, \uadf8\ub9ac\uace0 \uae34 \uc0dd\uc0b0 \uc218\uba85\uc774 \uc8fc\uc694 \uc694\uad6c \uc0ac\ud56d\uc77c \uacbd\uc6b0 D2\uac00 \ub354 \ub098\uc740 \uc120\ud0dd\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ub354\uc6b1 \uacac\uace0\ud558\uace0 \uc0ac\uc6a9\ud558\uae30 \uc26c\uc6b4 \ub3c4\uad6c\ub97c \uc6d0\ud558\uc2dc\uba74 A2\ub97c \uc120\ud0dd\ud558\uc138\uc694.<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">A2\ub294 \ub0b4\ucda9\uaca9\uc131, \ub0b4\uade0\uc5f4\uc131, \uac00\uacf5 \uc6a9\uc774\uc131 \ubc0f \ub0ae\uc740 \uc81c\uc791 \ub09c\uc774\ub3c4\uac00 \ub354 \uc911\uc694\ud55c \uacbd\uc6b0 \ub354 \uc548\uc804\ud55c \uc120\ud0dd\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\uad00\ub828 \ud398\uc774\uc9c0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>D2 \ube44\uad50:<\/strong> <a href=\"https:\/\/aobosteel.com\/ko\/d2-vs-m2-tool-steel\/\">D2 vs M2<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/d2-steel-vs-4140\/\">D2 \ub300 4140<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/o1-vs-d2-tool-steel\/\">D2 vs O1<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/dc53-vs-d2-tool-steel\/\">D2 vs DC53<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/d2-vs-d3-tool-steel\/\">D2 vs D3<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/d2-steel-vs-440c\/\">D2 vs 440C<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/d2-vs-s7-tool-steel\/\">D2 vs S7<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>\ucc38\uace0 \ud398\uc774\uc9c0:<\/strong> <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-heat-treatment-guide\/\">\uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-machining-allowance-chart\/\">\uacf5\uad6c\uac15 \uac00\uacf5 \uc5ec\uc720 \ucc28\ud2b8<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>\ud559\ub144\ubcc4 \uac00\uc871:<\/strong> <a href=\"https:\/\/aobosteel.com\/ko\/tool-steels\/\">\uacf5\uad6c\uac15 \ub4f1\uae09<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/d-series-tool-steels\/\">D\uacc4\uc5f4 \uacf5\uad6c\uac15<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-material-finder\/\">\uacf5\uad6c\uac15 \uc7ac\uc9c8 \ucc3e\uae30<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc870\uc131 \ubc94\uc704, \uacbd\ub3c4 \uc218\uce58 \ubc0f \uacbd\ud654\ub2a5 \ub370\uc774\ud130\ub294 D2 \/ 1.2379 \/ SKD11 \ubc0f A2 \/ 1.2363\uc5d0 \ub300\ud574 \uc77c\ubc18\uc801\uc73c\ub85c \uacf5\uac1c\ub41c \uac12\uc785\ub2c8\ub2e4. \ub0a9\ud488\ub41c \ub85c\ud2b8\uc758 \ubc00 \uc778\uc99d\uc11c\uc640 \ub300\uc870\ud558\uc5ec \uc815\ud655\ud55c \ubc94\uc704\ub97c \ud655\uc778\ud558\uc2ed\uc2dc\uc624.<\/p>","protected":false},"excerpt":{"rendered":"<p>D2 vs A2 Tool Steel: Practical Selection Guide D2 tool steel and A2 tool steel are both air-hardening cold-work tool steels, but they solve different tooling problems. D2 is the better choice when abrasive wear, edge retention, and long production life matter most. A2 is the better choice when chipping resistance, cracking resistance, easier machining, [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":15036,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"disabled","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-13242","page","type-page","status-publish","has-post-thumbnail","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.7 (Yoast SEO v28.7) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>D2 vs A2 Tool Steel: Wear Resistance or Chipping Risk?<\/title>\n<meta name=\"description\" content=\"D2 resists abrasive wear longer, A2 chips less and machines easier. Choose D2 for long abrasive runs and A2 for complex tools. Both run 58 to 60 HRC.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/d2-vs-a2-tool-steel\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"D2 vs A2 Tool Steel: Wear, Chipping &amp; Selection Guide\" \/>\n<meta property=\"og:description\" content=\"D2 resists abrasive wear longer, A2 chips less and machines easier. Choose D2 for long abrasive runs and A2 for complex tools. Both run 58 to 60 HRC.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/d2-vs-a2-tool-steel\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-16T04:25:33+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif\" \/>\n\t<meta property=\"og:image:width\" content=\"1254\" \/>\n\t<meta property=\"og:image:height\" content=\"1254\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"6\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"D2 vs A2 Tool Steel: Wear, Chipping &amp; Selection Guide\",\"datePublished\":\"2026-03-04T00:33:30+00:00\",\"dateModified\":\"2026-10-16T04:25:33+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/\"},\"wordCount\":1052,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/D2-VS-A2-AD-1.avif\",\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/\",\"name\":\"D2 vs A2 Tool Steel: Wear Resistance or Chipping Risk?\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/D2-VS-A2-AD-1.avif\",\"datePublished\":\"2026-03-04T00:33:30+00:00\",\"dateModified\":\"2026-10-16T04:25:33+00:00\",\"description\":\"D2 resists abrasive wear longer, A2 chips less and machines easier. Choose D2 for long abrasive runs and A2 for complex tools. Both run 58 to 60 HRC.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/D2-VS-A2-AD-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/D2-VS-A2-AD-1.avif\",\"width\":1254,\"height\":1254},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/d2-vs-a2-tool-steel\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"D2 vs A2 Tool Steel: Wear, Chipping &amp; Selection Guide\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"D2 vs A2 \uacf5\uad6c\uac15, \ub0b4\ub9c8\ubaa8\uc131 \ub610\ub294 \uce69\ud551 \uc704\ud5d8","description":"D2\ub294 \ub0b4\ub9c8\ubaa8\uc131\uc774 \ub354 \ub192\uace0 A2\ub294 \uce69\ud551\uc774 \uc801\uace0 \uac00\uacf5\uc774 \uc27d\uc2b5\ub2c8\ub2e4. \uc7a5\uae30\uac04 \ub9c8\ubaa8\uac00 \uc2ec\ud55c \uc791\uc5c5\uc5d0\ub294 D2\ub97c, \ubcf5\uc7a1\ud55c \ud615\uc0c1\uc758 \uacf5\uad6c\uc5d0\ub294 A2\ub97c \uc120\ud0dd\ud558\uc2ed\uc2dc\uc624. \ub450 \uac15\uc885 \ubaa8\ub450 \uc77c\ubc18\uc801\uc73c\ub85c 58-60 HRC\ub85c \uc0ac\uc6a9\ud569\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/d2-vs-a2-tool-steel\/","og_locale":"ko_KR","og_type":"article","og_title":"D2 vs A2 Tool Steel: Wear, Chipping &amp; Selection Guide","og_description":"D2 resists abrasive wear longer, A2 chips less and machines easier. Choose D2 for long abrasive runs and A2 for complex tools. Both run 58 to 60 HRC.","og_url":"https:\/\/aobosteel.com\/ko\/d2-vs-a2-tool-steel\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-16T04:25:33+00:00","og_image":[{"width":1254,"height":1254,"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif","type":"image\/png"}],"twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"6\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"D2 vs A2 Tool Steel: Wear, Chipping &amp; Selection Guide","datePublished":"2026-03-04T00:33:30+00:00","dateModified":"2026-10-16T04:25:33+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/"},"wordCount":1052,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif","inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/","url":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/","name":"D2 vs A2 \uacf5\uad6c\uac15, \ub0b4\ub9c8\ubaa8\uc131 \ub610\ub294 \uce69\ud551 \uc704\ud5d8","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif","datePublished":"2026-03-04T00:33:30+00:00","dateModified":"2026-10-16T04:25:33+00:00","description":"D2\ub294 \ub0b4\ub9c8\ubaa8\uc131\uc774 \ub354 \ub192\uace0 A2\ub294 \uce69\ud551\uc774 \uc801\uace0 \uac00\uacf5\uc774 \uc27d\uc2b5\ub2c8\ub2e4. \uc7a5\uae30\uac04 \ub9c8\ubaa8\uac00 \uc2ec\ud55c \uc791\uc5c5\uc5d0\ub294 D2\ub97c, \ubcf5\uc7a1\ud55c \ud615\uc0c1\uc758 \uacf5\uad6c\uc5d0\ub294 A2\ub97c \uc120\ud0dd\ud558\uc2ed\uc2dc\uc624. \ub450 \uac15\uc885 \ubaa8\ub450 \uc77c\ubc18\uc801\uc73c\ub85c 58-60 HRC\ub85c \uc0ac\uc6a9\ud569\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/"]}]},{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif","width":1254,"height":1254},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/d2-vs-a2-tool-steel\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"D2 vs A2 Tool Steel: Wear, Chipping &amp; Selection Guide"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif",1254,1254,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-150x150.avif",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-300x300.avif",300,300,true],"medium_large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-768x768.avif",768,768,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-1024x1024.avif",1024,1024,true],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif",1254,1254,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif",1254,1254,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-12x12.avif",12,12,true]},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"D2 vs A2 Tool Steel: Practical Selection Guide D2 tool steel and A2 tool steel are both air-hardening cold-work tool steels, but they solve different tooling problems. D2 is the better choice when abrasive wear, edge retention, and long production life matter most. A2 is the better choice when chipping resistance, cracking resistance, easier machining,&hellip;","rttpg_featured_image_url":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif",1254,1254,false],"landscape":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif",1254,1254,false],"portraits":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif",1254,1254,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-150x150.avif",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-300x300.avif",300,300,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-1024x1024.avif",1024,1024,true],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif",1254,1254,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1.avif",1254,1254,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/D2-VS-A2-AD-1-12x12.avif",12,12,true]},"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"D2 vs A2 Tool Steel: Practical Selection Guide D2 tool steel and A2 tool steel are both air-hardening cold-work tool steels, but they solve different tooling problems. D2 is the better choice when abrasive wear, edge retention, and long production life matter most. A2 is the better choice when chipping resistance, cracking resistance, easier machining,&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/13242","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=13242"}],"version-history":[{"count":6,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/13242\/revisions"}],"predecessor-version":[{"id":23072,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/13242\/revisions\/23072"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media\/15036"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=13242"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}