{"id":12368,"date":"2026-01-22T20:01:06","date_gmt":"2026-01-22T12:01:06","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=12368"},"modified":"2026-09-23T15:53:15","modified_gmt":"2026-09-23T07:53:15","slug":"selection-of-tool-steel-for-high-pressure-die-casting-dies","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/","title":{"rendered":"HPDC \uacf5\uad6c\uac15 \uc120\uc815 \uac00\uc774\ub4dc | H13 H11 \uacf5\uae09\uc5c5\uccb4 | \uc544\uc624\ubcf4 \uc2a4\ud2f8"},"content":{"rendered":"<section class=\"aobo-hpdc-dies-page\">\n  <style>\n\n    .aobo-hpdc-dies-page {\n      --aobo-blue: #0c56d0;\n      --aobo-blue-soft: #eaf2ff;\n      --aobo-border: #d7e5fb;\n      --aobo-text: #203044;\n      --aobo-muted: #617087;\n      --aobo-orange: #f59b23;\n      --aobo-shadow: 0 18px 45px rgba(12, 86, 208, 0.10);\n      font-family: inherit;\n      color: var(--aobo-text);\n      line-height: 1.7;\n      background: transparent;\n      padding: 0;\n      box-sizing: border-box;\n    }\n\n    .aobo-hpdc-dies-page * {\n      box-sizing: border-box;\n    }\n\n    .aobo-hpdc-dies-page .aobo-wrap {\n      max-width: 1180px;\n      margin: 0 auto;\n      padding: 0;\n    }\n\n    .aobo-hpdc-dies-page .aobo-hero {\n      background: linear-gradient(135deg, #ffffff 0%, #f7fbff 56%, #eaf2ff 100%);\n      border: 1px solid var(--aobo-border);\n      border-radius: 28px;\n      padding: 42px 38px;\n      margin-bottom: 24px;\n      box-shadow: var(--aobo-shadow);\n      overflow: hidden;\n      position: relative;\n    }\n\n    .aobo-hpdc-dies-page .aobo-hero::after {\n      content: \"\";\n      position: absolute;\n      right: -90px;\n      top: -90px;\n      width: 260px;\n      height: 260px;\n      border-radius: 50%;\n      background: rgba(12, 86, 208, 0.08);\n    }\n\n    .aobo-hpdc-dies-page .aobo-hero h1 {\n      margin: 0 0 16px;\n      color: #082d6f;\n      font-size: clamp(34px, 4vw, 54px);\n      line-height: 1.05;\n      letter-spacing: 0;\n      position: relative;\n      z-index: 2;\n    }\n\n    .aobo-hpdc-dies-page .aobo-hero p {\n      margin: 0 0 12px;\n      font-size: 17px;\n      color: #314158;\n      position: relative;\n      z-index: 2;\n    }\n\n    .aobo-hpdc-dies-page .aobo-article {\n      max-width: 1180px;\n      margin: 0 auto;\n    }\n\n    .aobo-hpdc-dies-page .aobo-btn {\n      display: inline-flex;\n      align-items: center;\n      justify-content: center;\n      min-height: 42px;\n      padding: 10px 16px;\n      border-radius: 999px;\n      text-align: center;\n      text-decoration: none;\n      font-weight: 700;\n      font-size: 14px;\n      line-height: 1.2;\n      transition: all 0.2s ease;\n      cursor: pointer;\n      white-space: nowrap;\n    }\n\n    .aobo-hpdc-dies-page .aobo-btn-primary {\n      background: var(--aobo-blue);\n      color: #ffffff !important;\n      border: 1px solid var(--aobo-blue);\n    }\n\n    .aobo-hpdc-dies-page .aobo-btn-secondary {\n      background: #ffffff;\n      color: var(--aobo-blue) !important;\n      border: 1px solid var(--aobo-border);\n    }\n\n    .aobo-hpdc-dies-page .aobo-btn:hover {\n      transform: translateY(-1px);\n    }\n\n    .aobo-hpdc-dies-page .aobo-supply-block {\n      display: grid;\n      grid-template-columns: auto minmax(0, 1fr);\n      align-items: center;\n      gap: 24px;\n      margin: 0 0 26px;\n      border: 1px solid var(--aobo-border);\n      border-radius: 24px;\n      background: #ffffff;\n      box-shadow: 0 14px 36px rgba(12, 86, 208, 0.09);\n      overflow: hidden;\n      padding: 24px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-supply-image {\n      width: 190px;\n      aspect-ratio: 1;\n      border: 1px solid var(--aobo-border);\n      border-radius: 18px;\n      overflow: hidden;\n      background: #f7fbff;\n    }\n\n    .aobo-hpdc-dies-page .aobo-supply-image img {\n      display: block;\n      width: 100%;\n      height: 100%;\n      object-fit: cover;\n    }\n\n    .aobo-hpdc-dies-page .aobo-supply-content {\n      display: flex;\n      flex-direction: column;\n      justify-content: center;\n      padding: 0;\n    }\n\n    .aobo-hpdc-dies-page .aobo-supply-content p {\n      margin: 0;\n      font-size: 17px;\n      color: var(--aobo-text);\n    }\n\n    .aobo-hpdc-dies-page .aobo-supply-actions {\n      display: flex;\n      flex-wrap: wrap;\n      gap: 12px;\n      margin-top: 18px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-supply-actions .aobo-btn {\n      min-width: 190px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-article h2 {\n      margin: 44px 0 16px;\n      color: #082d6f;\n      font-size: 30px;\n      line-height: 1.25;\n    }\n\n    .aobo-hpdc-dies-page .aobo-article h3 {\n      margin: 30px 0 12px;\n      color: #082d6f;\n      font-size: 23px;\n      line-height: 1.3;\n    }\n\n    .aobo-hpdc-dies-page .aobo-article p {\n      margin: 0 0 18px;\n      font-size: 17px;\n      color: var(--aobo-text);\n    }\n\n    .aobo-hpdc-dies-page .aobo-table-wrap {\n      overflow-x: auto;\n      margin: 22px 0 28px;\n      border-radius: 18px;\n      border: 1px solid var(--aobo-border);\n      box-shadow: 0 12px 32px rgba(12, 86, 208, 0.07);\n    }\n\n    .aobo-hpdc-dies-page .aobo-table {\n      width: 100%;\n      min-width: 760px;\n      border-collapse: collapse;\n      background: #ffffff;\n    }\n\n    .aobo-hpdc-dies-page .aobo-table th {\n      background: var(--aobo-blue-soft);\n      color: #082d6f;\n      text-align: left;\n      padding: 14px 16px;\n      font-size: 15px;\n      vertical-align: top;\n    }\n\n    .aobo-hpdc-dies-page .aobo-table td {\n      padding: 14px 16px;\n      border-bottom: 1px solid #e8eef8;\n      vertical-align: top;\n      font-size: 15px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-table tr:last-child td {\n      border-bottom: none;\n    }\n\n    .aobo-hpdc-dies-page .aobo-table td:first-child {\n      color: #082d6f;\n      font-weight: 700;\n    }\n\n    .aobo-hpdc-dies-page .aobo-note-box {\n      margin: 34px 0;\n      padding: 22px 24px;\n      border: 1px solid var(--aobo-border);\n      border-left: 5px solid var(--aobo-orange);\n      border-radius: 16px;\n      background: #fbfdff;\n      color: var(--aobo-muted);\n    }\n\n    .aobo-hpdc-dies-page .aobo-note-box p {\n      margin: 0 0 14px;\n      color: var(--aobo-muted);\n      font-style: italic;\n    }\n\n    .aobo-hpdc-dies-page .aobo-note-box p:last-child {\n      margin-bottom: 0;\n    }\n\n    .aobo-hpdc-dies-page .aobo-final-cta {\n      margin-top: 34px;\n      padding: 34px;\n      border-radius: 28px;\n      background: linear-gradient(135deg, #073b91 0%, #0c56d0 100%);\n      color: #ffffff;\n      box-shadow: 0 18px 45px rgba(12, 86, 208, 0.20);\n      display: flex;\n      align-items: center;\n      justify-content: space-between;\n      gap: 20px;\n      flex-wrap: wrap;\n    }\n\n    .aobo-hpdc-dies-page .aobo-final-cta h2 {\n      margin: 0 0 12px;\n      color: #ffffff;\n      font-size: 26px;\n      line-height: 1.25;\n      letter-spacing: 0;\n    }\n\n    .aobo-hpdc-dies-page .aobo-final-cta p {\n      margin: 0;\n      color: rgba(255, 255, 255, 0.92);\n      max-width: 760px;\n      font-size: 17px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-final-cta .aobo-supply-actions {\n      margin-top: 0;\n    }\n\n    .aobo-hpdc-dies-page .aobo-final-cta .aobo-btn-primary {\n      background: #ffffff;\n      border-color: #ffffff;\n      color: var(--aobo-blue) !important;\n    }\n\n    .aobo-hpdc-dies-page .aobo-final-cta .aobo-btn-primary:hover {\n      background: #fff7ed;\n      color: #073b91 !important;\n    }\n\n    .aobo-hpdc-dies-page .aobo-final-cta .aobo-btn-secondary {\n      background: transparent;\n      border-color: rgba(255, 255, 255, 0.75);\n      color: #ffffff !important;\n    }\n\n    .aobo-hpdc-dies-page .aobo-final-cta .aobo-btn-secondary:hover {\n      background: rgba(255, 255, 255, 0.14);\n      border-color: #ffffff;\n      color: #ffffff !important;\n    }\n\n    .aobo-hpdc-dies-page .aobo-image-marker {\n      margin: 26px 0 10px;\n      padding: 18px 20px;\n      border: 1px dashed var(--aobo-border);\n      border-radius: 14px;\n      background: #fbfdff;\n      color: var(--aobo-muted);\n      font-weight: 700;\n    }\n\n    .aobo-hpdc-dies-page .aobo-figure {\n      margin: 26px auto 34px;\n      max-width: 860px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-figure img {\n      display: block;\n      width: 100%;\n      height: auto;\n      border: 1px solid var(--aobo-border);\n      border-radius: 18px;\n      box-shadow: 0 12px 32px rgba(12, 86, 208, 0.07);\n      background: #ffffff;\n    }\n\n    .aobo-hpdc-dies-page .aobo-figure figcaption {\n      margin-top: 12px;\n      color: var(--aobo-muted);\n      font-size: 15px;\n      line-height: 1.6;\n    }\n\n    .aobo-hpdc-dies-page .aobo-figure figcaption strong {\n      display: block;\n      margin-bottom: 6px;\n      color: #082d6f;\n      font-size: 18px;\n      text-align: center;\n    }\n\n    .aobo-hpdc-dies-page .aobo-article a, .aobo-hpdc-dies-page .aobo-hero a {\n      color: var(--aobo-blue);\n      font-weight: 700;\n      text-decoration: none;\n    }\n\n    .aobo-hpdc-dies-page .aobo-article a:hover, .aobo-hpdc-dies-page .aobo-hero a:hover {\n      color: var(--aobo-orange);\n    }\n\n    @media (max-width: 760px) {\n    .aobo-hpdc-dies-page .aobo-hero {\n        padding: 30px 22px;\n      }\n\n    .aobo-hpdc-dies-page .aobo-hero h1 {\n        font-size: 34px;\n      }\n\n    .aobo-hpdc-dies-page .aobo-article h2 {\n        font-size: 25px;\n      }\n\n    .aobo-hpdc-dies-page .aobo-supply-block {\n        grid-template-columns: 1fr;\n        gap: 18px;\n        padding: 20px;\n      }\n\n    .aobo-hpdc-dies-page .aobo-supply-image {\n        width: min(190px, 100%);\n        margin: 0 auto;\n      }\n\n    .aobo-hpdc-dies-page .aobo-supply-content {\n        padding: 0;\n      }\n\n    .aobo-hpdc-dies-page .aobo-final-cta {\n        padding: 26px 22px;\n      }\n\n    .aobo-hpdc-dies-page .aobo-final-cta .aobo-supply-actions {\n        width: 100%;\n      }\n\n    .aobo-hpdc-dies-page .aobo-final-cta .aobo-btn {\n        width: 100%;\n      }\n    }\n\n    .aobo-hpdc-dies-page .aobo-grade-card {\n      margin: 26px 0;\n      padding: 26px 26px 24px;\n      border: 1px solid var(--aobo-border);\n      border-radius: 22px;\n      background: #ffffff;\n      box-shadow: 0 12px 32px rgba(12, 86, 208, 0.07);\n    }\n\n    .aobo-hpdc-dies-page .aobo-grade-card h3 {\n      margin: 0 0 12px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-grade-card p {\n      margin: 0 0 12px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-grade-card p:last-child {\n      margin-bottom: 0;\n    }\n\n    .aobo-hpdc-dies-page .aobo-cta-row {\n      display: flex;\n      flex-wrap: wrap;\n      align-items: center;\n      gap: 12px;\n      margin-top: 20px;\n    }\n\n    .aobo-hpdc-dies-page .aobo-cta-row > div {\n      display: contents;\n    }\n\n    .aobo-hpdc-dies-page .aobo-cta-row .aobo-btn {\n      min-width: 220px;\n    }\n\n    @media (max-width: 760px) {\n      .aobo-hpdc-dies-page .aobo-grade-card {\n        padding: 20px;\n      }\n\n      .aobo-hpdc-dies-page .aobo-cta-row .aobo-btn {\n        width: 100%;\n        min-width: 0;\n      }\n    }\n\n    @media (max-width: 520px) {\n      .aobo-hpdc-dies-page .aobo-table th,\n      .aobo-hpdc-dies-page .aobo-table td {\n        padding: 11px 12px;\n        font-size: 14px;\n      }\n    }\n    <\/style>\n\n  <div class=\"aobo-wrap\">\n    <header class=\"aobo-hero\">\n      <h1 id=\"h-selection-of-tool-steel-for-high-pressure-die-casting-dies\">\uace0\uc555 \ub2e4\uc774\uce90\uc2a4\ud305 \uae08\ud615\uc6a9 \uacf5\uad6c\uac15 \uc120\uc815<\/h1>\n      <p>\uace0\uc555 \ub2e4\uc774\uce90\uc2a4\ud305(HPDC)\uc740 \uc6a9\uc735 \uae08\uc18d\uc744 6.9~206.8 MPa(1,000~30,000 psi)\uc758 \uc555\ub825\uc73c\ub85c \uac15\ucca0 \uae08\ud615\uc5d0 \uc8fc\uc785\ud558\ub294 \uace0\uc18d \uacf5\uc815\uc785\ub2c8\ub2e4. \uae08\ud615 \ub0b4\ubd80 \uacf5\uac04\uc740 \uc218 \ucd08 \ub9cc\uc5d0 \ucc44\uc6cc\uc9c0\uace0 \uc751\uace0\ub418\uba70, \uc774 \uacfc\uc815\uc5d0\uc11c \uae08\ud615 \ud45c\uba74\uc740 \ubc18\ubcf5\uc801\uc778 \uc5f4\uc801 \ubc0f \uae30\uacc4\uc801 \ud558\uc911\uc744 \ubc1b\uac8c \ub429\ub2c8\ub2e4.<\/p>\n      <p>\uac01 \uc0ac\uc774\ud074 \ub3d9\uc548 \uae08\ud615 \ud45c\uba74\uc740 \uc6a9\uc735 \ud569\uae08\uacfc \uc811\ucd09\ud558\uba74\uc11c \uae09\uc18d\ud558\uac8c \uac00\uc5f4\ub41c \ud6c4 \ubd80\ud488 \ubc30\ucd9c \uc2dc \ub0c9\uac01\ub429\ub2c8\ub2e4. \uc774\ub85c \uc778\ud574 \uc8fc\uae30\uc801\uc778 \uc555\ucd95 \ubc0f \uc778\uc7a5 \uc751\ub825\uc774 \ubc1c\uc0dd\ud569\ub2c8\ub2e4. \ub3d9\uc2dc\uc5d0 \uace0\uc18d \uae08\uc18d \ud750\ub984\uc740 \ud45c\uba74 \uce68\uc2dd\uc744 \uc720\ubc1c\ud558\uace0, \uc6a9\uc735 \ud569\uae08\uacfc \uae08\ud615 \uc0ac\uc774\uc758 \ud654\ud559\uc801 \ubc18\uc751\uc740 \ub0a9\ub55c \ud604\uc0c1\uc744 \ucd08\ub798\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n      <p>\uc2e4\uc81c\ub85c \ub2e4\uc774\uc758 \uc218\uba85\uc740 \uc2e4\uc81c \uc791\ub3d9 \uc870\uac74\uc5d0\uc11c \uc5b4\ub5a4 \uace0\uc7a5 \uba54\ucee4\ub2c8\uc998(\uc5f4 \ud53c\ub85c, \uce68\uc2dd \ub610\ub294 \ub0a9\ub55c)\uc774 \uc9c0\ubc30\uc801\uc778\uc9c0\uc5d0 \ub530\ub77c \uacb0\uc815\ub429\ub2c8\ub2e4.<\/p>\n    <\/header>\n\n    <main class=\"aobo-article\">\n      <h2>\uc120\ud0dd \uc694\uc778<\/h2>\n      <p>HPDC\uc6a9 \uacf5\uad6c\uac15\uc744 \uc120\ud0dd\ud560 \ub54c\ub294 \uba3c\uc800 \uc8fc\uc694 \ud30c\uc190 \ubaa8\ub4dc\ub97c \ud30c\uc545\ud55c \ub2e4\uc74c, \uadf8 \ubaa8\ub4dc\uc5d0 \uc800\ud56d\ud560 \uc218 \uc788\ub294 \uc7ac\uc9c8\uc744 \uc120\ud0dd\ud558\ub294 \uac83\uc774 \uc911\uc694\ud569\ub2c8\ub2e4.<\/p>\n      <p>\uc5f4\ud53c\ub85c(\uc5f4\uade0\uc5f4)\ub294 \uac00\uc7a5 \ud754\ud55c \uace0\uc7a5 \uc6d0\uc778\uc785\ub2c8\ub2e4. \ubc18\ubcf5\uc801\uc778 \uac00\uc5f4\uacfc \ub0c9\uac01\uc73c\ub85c \uc778\ud574 \ud45c\uba74\uc5d0 \uade0\uc5f4\uc774 \ubc1c\uc0dd\ud558\uace0, \uc774 \uade0\uc5f4\uc740 \uae30\uacc4\uc801 \uc751\ub825 \ud558\uc5d0\uc11c \uc804\ud30c\ub418\uc5b4 \uacb0\uad6d \ubc15\ub9ac \ub610\ub294 \ud30c\uc190\uc73c\ub85c \uc774\uc5b4\uc9d1\ub2c8\ub2e4.<\/p>\n      <p>\uc774\ub7ec\ud55c \uacfc\uc815\uc744 \uc9c0\uc5f0\uc2dc\ud0a4\uae30 \uc704\ud574\uc11c\ub294 \uac15\ucca0\uc774 \uace0\uc628\uc5d0\uc11c\ub3c4 \uac15\ub3c4\ub97c \uc720\uc9c0\ud574\uc57c \ud558\uba70, \uc774\ub294 \ubc18\ubcf5\uc801\uc778 \uac00\uc5f4 \uacfc\uc815\uc5d0\uc11c \ubc1c\uc0dd\ud558\ub294 \ud15c\ud37c \uc5f0\ud654\uc5d0 \uc800\ud56d\ud574\uc57c \ud568\uc744 \uc758\ubbf8\ud569\ub2c8\ub2e4. \ub3d9\uc2dc\uc5d0, \uade0\uc5f4\uc774 \ubc1c\uc0dd\ud588\uc744 \ub54c \uade0\uc5f4 \uc804\ud30c \uc18d\ub3c4\ub97c \ub2a6\ucd94\uae30 \uc704\ud574\uc11c\ub294 \ucda9\ubd84\ud55c \uc778\uc131\uc774 \ud544\uc694\ud569\ub2c8\ub2e4.<\/p>\n      <p>\uc774\ub7ec\ud55c \uc694\uad6c\uc0ac\ud56d\ub4e4\uc740 \uc2e4\uc81c\ub85c\ub294 \uc0c1\ucda9\ub429\ub2c8\ub2e4. \uacbd\ub3c4\ub97c \ub192\uc774\uba74 \uce68\uc2dd \ubc0f \ubcc0\ud615\uc5d0 \ub300\ud55c \uc800\ud56d\uc131\uc740 \ud5a5\uc0c1\ub418\uc9c0\ub9cc \uade0\uc5f4 \uc131\uc7a5\uc774 \uac00\uc18d\ud654\ub429\ub2c8\ub2e4. \uc778\uc131\uc744 \ub192\uc774\uba74 \uade0\uc5f4 \uc800\ud56d\uc131\uc740 \ud5a5\uc0c1\ub418\uc9c0\ub9cc \uace0\uc628 \uac15\ub3c4\uc640 \ub0b4\ub9c8\ubaa8\uc131\uc740 \uc800\ud558\ub429\ub2c8\ub2e4.<\/p>\n      <p>\uc0dd\uc0b0 \uacfc\uc815\uc5d0\uc11c \uc774\ub7ec\ud55c \uade0\ud615\uc740 \ud2b9\uc815 \uc18d\uc131 \ud558\ub098\ub97c \uadf9\ub300\ud654\ud558\ub294 \uac83\uc774 \uc544\ub2c8\ub77c, \uc791\uc5c5 \uac00\ub2a5\ud55c \ubc94\uc704 \ub0b4\uc5d0\uc11c \uacbd\ub3c4\ub97c \uc120\ud0dd\ud568\uc73c\ub85c\uc368 \uc8fc\ub85c \uc870\uc808\ub429\ub2c8\ub2e4.<\/p>\n      <h2>\ucd94\ucc9c \uacf5\uad6c\uac15<\/h2>\n      <div class=\"aobo-grade-card\">\n        <h3 id=\"h-h13-tool-steel-supplier-1-2344-skd61\">H13 \uacf5\uad6c\uac15 \uacf5\uae09\uc5c5\uccb4 | 1.2344 | SKD61<\/h3>\n        <p>H13\uc740 \ud2b9\uc815 \uace0\uc7a5 \ubaa8\ub4dc\uac00 \uc9c0\ubc30\uc801\uc774\uc9c0 \uc54a\uc740 \uc54c\ub8e8\ubbf8\ub284 \ubc0f \ub9c8\uadf8\ub124\uc298 HPDC\uc5d0 \ub300\ud55c \ud45c\uc900 \uc120\ud0dd\uc785\ub2c8\ub2e4.<\/p>\n        <p>\uc774 \ud569\uae08\uc740 \uc5f4\ucc98\ub9ac \uc5f0\ud654\uc5d0 \ub300\ud55c \uc548\uc815\uc801\uc778 \uc800\ud56d\uc131\uc744 \uc81c\uacf5\ud558\uc5ec \ubc18\ubcf5\uc801\uc778 \uc5f4 \uc21c\ud658\uc5d0\ub3c4 \uac15\ub3c4\ub97c \uc720\uc9c0\ud560 \uc218 \uc788\ub3c4\ub85d \ud569\ub2c8\ub2e4. \ub3d9\uc2dc\uc5d0, \uade0\uc5f4 \uc804\ud30c\ub97c \uc81c\uc5b4\ud560 \uc218 \uc788\ub294 \ucda9\ubd84\ud55c \uc778\uc131\uc744 \uac16\ucd94\uace0 \uc788\uc5b4 \uc5f4 \uade0\uc5f4 \uad00\ub9ac\uc5d0 \ub9e4\uc6b0 \uc911\uc694\ud569\ub2c8\ub2e4.<\/p>\n        <p>\uc77c\ubc18\uc801\uc73c\ub85c 42~52 HRC \ubc94\uc704\uc5d0\uc11c \uc0ac\uc6a9\ub418\ub294\ub370, \uc774 \ubc94\uc704\ub294 \uc5f4 \ud53c\ub85c \ubc0f \ud558\uc911 \ud558\uc5d0\uc11c\uc758 \uc18c\uc131 \ubcc0\ud615\uc5d0 \ub300\ud55c \uc77c\uad00\ub41c \uc800\ud56d\uc131\uc744 \uc81c\uacf5\ud558\uae30 \ub54c\ubb38\uc5d0 \ub110\ub9ac \ucc44\ud0dd\ub418\uace0 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n        <div class=\"aobo-cta-row\">\n          <div class=\"popmake-16052 hs-cta-trigger-button hs-cta-trigger-button-230288465624\"><a class=\"aobo-btn aobo-btn-primary\">\uc9c0\uae08 \ubc14\ub85c \ubb38\uc758\ud558\uc138\uc694<\/a><\/div>\n          <a class=\"aobo-btn aobo-btn-secondary\" href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel\/\">H13 \uc790\uc7ac \uacf5\uae09 \uc138\ubd80 \uc815\ubcf4\ub97c \ud655\uc778\ud558\uc138\uc694.<\/a>\n        <\/div>\n      <\/div>\n      <div class=\"aobo-grade-card\">\n        <h3 id=\"h-aisi-h11-tool-steel-1-2343-skd6\">AISI H11 \uacf5\uad6c\uac15 | 1.2343 | SKD6<\/h3>\n        <p>\uade0\uc5f4 \uc704\ud5d8\uc774 \ub9c8\ubaa8 \uc704\ud5d8\ubcf4\ub2e4 \ud074 \uacbd\uc6b0 H11\uc774 \uc120\ud638\ub429\ub2c8\ub2e4.<\/p>\n        <p>H13\uc5d0 \ube44\ud574 \uc778\uc131\uc774 \ub354 \ub192\uace0 \uc5f4\ucda9\uaca9 \uc800\ud56d\uc131\uc774 \uc6b0\uc218\ud558\uc5ec \uc751\ub825 \uc9d1\uc911\uc73c\ub85c \uade0\uc5f4 \ubc1c\uc0dd \uc704\ud5d8\uc774 \ub192\uc544\uc9c0\ub294 \ub300\ud615 \uae08\ud615\uc774\ub098 \ubcf5\uc7a1\ud55c \ud615\uc0c1\uc5d0 \ub354\uc6b1 \uc801\ud569\ud569\ub2c8\ub2e4.<\/p>\n        <p>\uc77c\ubc18\uc801\uc73c\ub85c 42~50 HRC\uc758 \uacbd\ub3c4\ub97c \uc0ac\uc6a9\ud569\ub2c8\ub2e4. \uacbd\ub3c4\uac00 \uc57d\uac04 \ub0ae\uc73c\uba74 \uade0\uc5f4 \uc804\ud30c\uc5d0 \ub300\ud55c \uc800\ud56d\uc131\uc774 \ud5a5\uc0c1\ub418\uc5b4 \uace0\uc751\ub825 \uc601\uc5ed\uc5d0\uc11c \uc0ac\uc6a9 \uc218\uba85\uc774 \uc5f0\uc7a5\ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n        <div class=\"aobo-cta-row\">\n          <div class=\"popmake-16052 hs-cta-trigger-button hs-cta-trigger-button-230288465624\"><a class=\"aobo-btn aobo-btn-primary\">\uc9c0\uae08 \ubc14\ub85c \ubb38\uc758\ud558\uc138\uc694<\/a><\/div>\n          <a class=\"aobo-btn aobo-btn-secondary\" href=\"https:\/\/aobosteel.com\/ko\/h11-tool-steel\/\">H11 \uc790\uc7ac \uacf5\uae09 \uc138\ubd80 \uc815\ubcf4\ub97c \ud655\uc778\ud558\uc138\uc694.<\/a>\n        <\/div>\n      <\/div>\n      <div class=\"aobo-grade-card\">\n        <h3 id=\"h-aisi-h21-tool-steel-1-2581-skd5\">AISI H21 \uacf5\uad6c\uac15 | 1.2581 | SKD5<\/h3>\n        <p>H21\uc740 \uc791\ub3d9 \uc628\ub3c4\uac00 \uc8fc\uc694 \uc81c\ud55c \uc694\uc18c\uc77c \ub54c \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/p>\n        <p>\ub192\uc740 \ud145\uc2a4\ud150 \ud568\ub7c9 \ub355\ubd84\uc5d0 H11 \ubc0f H13 \ud569\uae08\uc774 \uc5f0\ud654\ub418\uae30 \uc2dc\uc791\ud558\ub294 \uc628\ub3c4\uc5d0\uc11c\ub3c4 \uac15\ub3c4\ub97c \uc720\uc9c0\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ub530\ub77c\uc11c \uc5f4 \ubd80\ud558\uac00 \ud6e8\uc52c \ub192\uc740 \ud669\ub3d9 \ubc0f \uad6c\ub9ac \ub2e4\uc774\uce90\uc2a4\ud305\uc5d0 \uc801\ud569\ud569\ub2c8\ub2e4.<\/p>\n        <p>\ub2e8\uc810\uc740 \uc778\uc131\uc774 \ub0ae\uace0 \uc5f4\ucda9\uaca9\uc5d0 \ub300\ud55c \ubbfc\uac10\ub3c4\uac00 \ub192\ub2e4\ub294 \uac83\uc785\ub2c8\ub2e4. \uc77c\ubc18\uc801\uc73c\ub85c \ucde8\uc131 \ud30c\uad34 \uc704\ud5d8\uc744 \uc904\uc774\uae30 \uc704\ud574 38~42 HRC\uc5d0\uc11c \uc0ac\uc6a9\ub418\uba70, \ubd80\uc801\uc808\ud55c \ub0c9\uac01\uc740 \uade0\uc5f4 \ubc1c\uc0dd\uc744 \ud06c\uac8c \uc99d\uac00\uc2dc\ud0ac \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n        <div class=\"aobo-cta-row\">\n          <div class=\"popmake-16052 hs-cta-trigger-button hs-cta-trigger-button-230288465624\"><a class=\"aobo-btn aobo-btn-primary\">\uc9c0\uae08 \ubc14\ub85c \ubb38\uc758\ud558\uc138\uc694<\/a><\/div>\n          <a class=\"aobo-btn aobo-btn-secondary\" href=\"https:\/\/aobosteel.com\/ko\/h21-tool-steel\/\">H21 \uc790\uc7ac \uacf5\uae09 \uc0c1\uc138 \uc815\ubcf4\ub97c \ud655\uc778\ud558\uc138\uc694.<\/a>\n        <\/div>\n      <\/div>\n      <div class=\"aobo-grade-card\">\n        <h3 id=\"h-aisi-p20-tool-steel-1-2311-3cr2mo\">AISI P20 \uacf5\uad6c\uac15 | 1.2311 | 3Cr2Mo<\/h3>\n        <p>P20\uc740 \uc5f4 \ubd80\ud558\uac00 \ube44\uad50\uc801 \ub0ae\uc740 \uc544\uc5f0 \ub2e4\uc774\uce90\uc2a4\ud305\uc5d0\ub9cc \uace0\ub824\ud574\uc57c \ud569\ub2c8\ub2e4.<\/p>\n        <p>\uc774 \uc18c\uc7ac\ub294 \uc0ac\uc804 \uacbd\ud654 \ucc98\ub9ac\ub41c \uac15\ucca0(28~37 HRC)\uc774\ubbc0\ub85c \ucd94\uac00 \uc5f4\ucc98\ub9ac \uc5c6\uc774 \ucd5c\uc885 \uce58\uc218\ub85c \uc9c1\uc811 \uac00\uacf5\ud560 \uc218 \uc788\uc5b4 \ubcc0\ud615 \uc704\ud5d8\uacfc \uc0dd\uc0b0 \uc2dc\uac04\uc744 \uc904\uc5ec\uc90d\ub2c8\ub2e4.<\/p>\n        <p>\ud558\uc9c0\ub9cc \uc54c\ub8e8\ubbf8\ub284\uc774\ub098 \ub9c8\uadf8\ub124\uc298 HPDC\uc5d0 \ud544\uc694\ud55c \uace0\uc628 \uac15\ub3c4\uac00 \ubd80\uc871\ud558\uc5ec \uadf8\ub7ec\ud55c \uc870\uac74\uc5d0\ub294 \uc801\ud569\ud558\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4.<\/p>\n        <div class=\"aobo-cta-row\">\n          <div class=\"popmake-16052 hs-cta-trigger-button hs-cta-trigger-button-230288465624\"><a class=\"aobo-btn aobo-btn-primary\">\uc9c0\uae08 \ubc14\ub85c \ubb38\uc758\ud558\uc138\uc694<\/a><\/div>\n          <a class=\"aobo-btn aobo-btn-secondary\" href=\"https:\/\/aobosteel.com\/ko\/p20-tool-steel\/\">P20 \uc790\uc7ac \uacf5\uae09 \uc138\ubd80 \uc815\ubcf4\ub97c \ud655\uc778\ud558\uc138\uc694.<\/a>\n        <\/div>\n      <\/div>\n      <h2>\uc694\uc57d\ud45c<\/h2>\n      <div class=\"aobo-table-wrap\">\n        <table class=\"aobo-table\">\n          <thead><tr><th>\uacf5\uad6c\uac15 \ub4f1\uae09<\/th><th>\uc77c\ubc18\uc801\uc778 \uacbd\ub3c4<\/th><th>HPDC\uc758 \uc8fc\uc694 \uc7a5\uc810<\/th><\/tr><\/thead>\n          <tbody>\n            <tr><td>AISI H13<\/td><td>42\u201352 HRC<\/td><td>\uc5f4\ud53c\ub85c, \uc5f0\ud654 \ubc0f \ubcc0\ud615\uc5d0 \ub300\ud55c \uade0\ud615 \uc7a1\ud78c \uc800\ud56d\uc131<\/td><\/tr>\n            <tr><td>AISI H11<\/td><td>42\u201350 HRC<\/td><td>\ub354 \ub192\uc740 \uc778\uc131; \uade0\uc5f4 \uc804\ud30c\uc5d0 \ub300\ud55c \ub354 \ub098\uc740 \uc800\ud56d\uc131<\/td><\/tr>\n            <tr><td>AISI H21<\/td><td>38\u201342 HRC<\/td><td>\uace0\uc628 \ud658\uacbd\uc5d0\uc11c\ub3c4 \uac15\ub3c4\ub97c \uc720\uc9c0\ud569\ub2c8\ub2e4.<\/td><\/tr>\n            <tr><td>AISI P20<\/td><td>28~37 HRC<\/td><td>\uc0ac\uc804 \uacbd\ud654 \ucc98\ub9ac\ub428; \uc800\uc628 \uc544\uc5f0 \ub2e4\uc774\uce90\uc2a4\ud305\uc5d0 \uc801\ud569<\/td><\/tr>\n          <\/tbody>\n        <\/table>\n      <\/div>\n    <\/main>\n  <\/div>\n<\/section>","protected":false},"excerpt":{"rendered":"<p>Selection of Tool Steel for High Pressure Die Casting Dies High-pressure die casting (HPDC) is a high-speed process in which molten metal is injected into a steel die under pressures of 6.9\u2013206.8 MPa (1,000\u201330,000 psi). The cavity fills and solidifies within seconds, exposing the die surface to repeated thermal and mechanical loading. During each cycle, [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-12368","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.6 (Yoast SEO v28.6) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>HPDC Tool Steel Selection Guide | H13 H11 Supplier | Aobo Steel<\/title>\n<meta name=\"description\" content=\"Select the right tool steel for HPDC dies based on failure modes. H13, H11, H21, and P20 are available for bulk supply with stable quality and MTC. Aobo Steel.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"HPDC Tool Steel Selection Guide | H13 H11 Supplier | Aobo Steel\" \/>\n<meta property=\"og:description\" content=\"Select the right tool steel for HPDC dies based on failure modes. H13, H11, H21, and P20 are available for bulk supply with stable quality and MTC. Aobo Steel.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-09-23T07:53:15+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"3\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/selection-of-tool-steel-for-high-pressure-die-casting-dies\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/selection-of-tool-steel-for-high-pressure-die-casting-dies\\\/\",\"name\":\"HPDC Tool Steel Selection Guide | H13 H11 Supplier | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-01-22T12:01:06+00:00\",\"dateModified\":\"2026-09-23T07:53:15+00:00\",\"description\":\"Select the right tool steel for HPDC dies based on failure modes. H13, H11, H21, and P20 are available for bulk supply with stable quality and MTC. Aobo Steel.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/selection-of-tool-steel-for-high-pressure-die-casting-dies\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/selection-of-tool-steel-for-high-pressure-die-casting-dies\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/selection-of-tool-steel-for-high-pressure-die-casting-dies\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"HPDC Tool Steel Selection Guide | H13 H11 Supplier | Aobo Steel\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"HPDC \uacf5\uad6c\uac15 \uc120\uc815 \uac00\uc774\ub4dc | H13 H11 \uacf5\uae09\uc5c5\uccb4 | \uc544\uc624\ubcf4 \uc2a4\ud2f8","description":"\uace0\uc7a5 \ubaa8\ub4dc\ub97c \uace0\ub824\ud558\uc5ec HPDC \uae08\ud615\uc5d0 \uc801\ud569\ud55c \uacf5\uad6c\uac15\uc744 \uc120\ud0dd\ud558\uc2ed\uc2dc\uc624. H13, H11, H21, P20\uc740 \uc548\uc815\uc801\uc778 \ud488\uc9c8\uacfc MTC\ub97c \uac16\ucd98 \uc81c\ud488\uc73c\ub85c \ub300\ub7c9 \uacf5\uae09 \uac00\ub2a5\ud569\ub2c8\ub2e4. \uc544\uc624\ubcf4\uac15.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/","og_locale":"ko_KR","og_type":"article","og_title":"HPDC Tool Steel Selection Guide | H13 H11 Supplier | Aobo Steel","og_description":"Select the right tool steel for HPDC dies based on failure modes. H13, H11, H21, and P20 are available for bulk supply with stable quality and MTC. Aobo Steel.","og_url":"https:\/\/aobosteel.com\/ko\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-09-23T07:53:15+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"3\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/","url":"https:\/\/aobosteel.com\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/","name":"HPDC \uacf5\uad6c\uac15 \uc120\uc815 \uac00\uc774\ub4dc | H13 H11 \uacf5\uae09\uc5c5\uccb4 | \uc544\uc624\ubcf4 \uc2a4\ud2f8","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-01-22T12:01:06+00:00","dateModified":"2026-09-23T07:53:15+00:00","description":"\uace0\uc7a5 \ubaa8\ub4dc\ub97c \uace0\ub824\ud558\uc5ec HPDC \uae08\ud615\uc5d0 \uc801\ud569\ud55c \uacf5\uad6c\uac15\uc744 \uc120\ud0dd\ud558\uc2ed\uc2dc\uc624. H13, H11, H21, P20\uc740 \uc548\uc815\uc801\uc778 \ud488\uc9c8\uacfc MTC\ub97c \uac16\ucd98 \uc81c\ud488\uc73c\ub85c \ub300\ub7c9 \uacf5\uae09 \uac00\ub2a5\ud569\ub2c8\ub2e4. \uc544\uc624\ubcf4\uac15.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"HPDC Tool Steel Selection Guide | H13 H11 Supplier | Aobo Steel"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Selection of Tool Steel for High Pressure Die Casting Dies High-pressure die casting (HPDC) is a high-speed process in which molten metal is injected into a steel die under pressures of 6.9\u2013206.8 MPa (1,000\u201330,000 psi). The cavity fills and solidifies within seconds, exposing the die surface to repeated thermal and mechanical loading. During each cycle,&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Selection of Tool Steel for High Pressure Die Casting Dies High-pressure die casting (HPDC) is a high-speed process in which molten metal is injected into a steel die under pressures of 6.9\u2013206.8 MPa (1,000\u201330,000 psi). The cavity fills and solidifies within seconds, exposing the die surface to repeated thermal and mechanical loading. During each cycle,&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/12368","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=12368"}],"version-history":[{"count":2,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/12368\/revisions"}],"predecessor-version":[{"id":19631,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/12368\/revisions\/19631"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=12368"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}