{"id":11688,"date":"2025-12-23T14:12:35","date_gmt":"2025-12-23T06:12:35","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=11688"},"modified":"2026-10-16T08:38:22","modified_gmt":"2026-10-16T00:38:22","slug":"m2-tool-steel-heat-treatment","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/m2-tool-steel-heat-treatment\/","title":{"rendered":"M2\uac15 \uc5f4\ucc98\ub9ac: \uacbd\ud654, \ud15c\ud37c\ub9c1 \ubc0f 60~65 HRC \uacbd\ub3c4\ud45c"},"content":{"rendered":"<h1 class=\"wp-block-heading\">M2 \uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \uacf5\uad6c\uac15\uc740 2\ub2e8 \uc608\uc5f4, 1190\u20131230\u00b0C\uc5d0\uc11c\uc758 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654, \uc624\uc77c\u00b7\uacf5\uae30 \ub610\ub294 \uc5fc\uc695 \ub2f4\uae08\uc9c8, \uadf8 \ud6c4 538\u2013595\u00b0C\uc5d0\uc11c 2\ud68c \ub610\ub294 3\ud68c \ub728\uc784\uc73c\ub85c \uc5f4\ucc98\ub9ac\ub429\ub2c8\ub2e4. \uc62c\ubc14\ub974\uac8c \ub728\uc784\ud558\uba74 M2\ub294 \uc57d 60\u201365 HRC\uc5d0 \ub3c4\ub2ec\ud558\uba70, \uace0\uc18d\ub3c4\uac15\uc5d0\uc11c \uae30\ub300\ub418\ub294 \ub192\uc740 \uacbd\ub3c4, \ub0b4\ub9c8\ubaa8\uc131 \ubc0f \uc801\uc5f4 \uacbd\ub3c4\ub97c \ub098\ud0c0\ub0c5\ub2c8\ub2e4. \ub728\uc784 \uc628\ub3c4\ubcc4 \uacbd\ub3c4 \uac12\uc740 \ud480\ub9bc \ubc0f \uc801\uc5f4 \uacbd\ub3c4 \ubc94\uc704\uc640 \ud568\uaed8 \ucc28\ud2b8\ub85c \uc81c\uc2dc\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. <a href=\"https:\/\/aobosteel.com\/ko\/m2-tool-steel-hardness\/\">M2 \uacf5\uad6c\uac15 \uacbd\ub3c4<\/a> \ud398\uc774\uc9c0.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc77c\ubc18\uc801\uc778 \uacf5\uc815 \uc21c\uc11c\ub294 540~650\u00b0C\uc5d0\uc11c 1\ucc28 \uc608\uc5f4 \ud6c4 845~870\u00b0C\uc5d0\uc11c 2\ucc28 \uc608\uc5f4\ud558\ub294 \uac83\uc785\ub2c8\ub2e4. \uc804\uccb4 \uc628\ub3c4\uac00 \uade0\uc77c\ud574\uc9c0\uba74 2~5\ubd84 \uc815\ub3c4 \uc9e7\uac8c \uc720\uc9c0\ud569\ub2c8\ub2e4. \uadf8\ub7f0 \ub2e4\uc74c 66~93\u00b0C\uae4c\uc9c0 \uae09\ub7ad\ud558\uace0 \uc989\uc2dc \ud15c\ud37c\ub9c1\ud569\ub2c8\ub2e4. \uacf5\uc815 \uac00\ub2a5 \ubc94\uc704\uac00 \uc881\uae30 \ub54c\ubb38\uc5d0 \uc544\ub798\uc758 \uc81c\uc5b4 \uc694\uc18c\ub4e4\uc774 \ub178 \uac00\uc5f4 \uc2dc\uac04\ubcf4\ub2e4 \ub354 \uc911\uc694\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">M2\ub294 \ubab0\ub9ac\ube0c\ub374-\ud145\uc2a4\ud150 \uace0\uc18d \uacf5\uad6c\uac15\uc785\ub2c8\ub2e4. \uacfc\ub3c4\ud55c \uc720\uc9c0 \uc2dc\uac04, \uacfc\uc5f4, \ubd80\uc801\uc808\ud55c \ubd84\uc704\uae30 \uc81c\uc5b4 \ub610\ub294 \uc9c0\uc5f0\ub418\uace0 \ubd88\ucda9\ubd84\ud55c \ud15c\ud37c\ub9c1\uc740 \uacbd\ub3c4 \uc800\ud558, \uacb0\uc815\ub9bd \uc870\ub300\ud654, \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8, \uade0\uc5f4, \ud45c\uba74 \ud0c8\ud0c4 \ub610\ub294 \uce58\uc218 \ubd88\uc548\uc815\uc131\uacfc \uac19\uc740 \ubb38\uc81c\ub97c \uc57c\uae30\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">M2 \uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \uc628\ub3c4\ud45c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc544\ub798 \ud45c\ub294 M2 \uacf5\uad6c\uac15\uc758 \uc8fc\uc694 \uc5f4\ucc98\ub9ac \ub370\uc774\ud130\ub97c \uc694\uc57d\ud55c \uac83\uc785\ub2c8\ub2e4. \uc804\uccb4 \uacf5\uc815 \uc21c\uc11c\ub294 \ub2e4\uc74c \ub2e8\uacc4\ubcc4 \uc124\uba85\uc5d0\uc11c \ud655\uc778\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ucc98\ub9ac \ub2e8\uacc4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc628\ub3c4\/\uc870\uac74<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud0a4 \ucee8\ud2b8\ub864<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b4\ub2d0\ub9c1<\/td><td class=\"has-text-align-left\" data-align=\"left\">870~900\u00b0C \/ 1600~1650\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub450\uaed8 1\uc778\uce58\ub2f9 \uc57d 1\uc2dc\uac04 \ub3d9\uc548 \uc720\uc9c0\ud569\ub2c8\ub2e4. \ub178\uc5d0\uc11c 650\u00b0C\uae4c\uc9c0 \ucc9c\ucc9c\ud788 \ub0c9\uac01\ud55c \ud6c4 \uacf5\ub7ad\ud569\ub2c8\ub2e4. \uc5b4\ub2d0\ub9c1 \ud6c4 \uacbd\ub3c4\ub294 \uc77c\ubc18\uc801\uc73c\ub85c \uc57d 241 HB\uc774\uba70, \uaddc\uaca9\uc0c1 \ucd5c\ub300 \uc57d 248 HB\uae4c\uc9c0 \uac00\ub2a5\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc2a4\ud2b8\ub808\uc2a4 \ud574\uc18c<\/td><td class=\"has-text-align-left\" data-align=\"left\">650~675\u00b0C \/ 1200~1245\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace0\uac15\ub3c4 \uac00\uacf5 \ud6c4 \uc0ac\uc6a9\ud569\ub2c8\ub2e4. \ub2e8\uba74\uc801 1\uc778\uce58\ub2f9 1~2\uc2dc\uac04 \ub3d9\uc548 \uc720\uc9c0\ud55c \ud6c4 \ucc9c\ucc9c\ud788 \uc2dd\ud788\uc2ed\uc2dc\uc624.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uccab \ubc88\uc9f8 \uc608\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">540~650\u00b0C \/ 1000~1200\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucd08\uae30 \uc5f4 \ucda9\uaca9\uc744 \uc904\uc5ec\uc90d\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub450 \ubc88\uc9f8 \uc608\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">845\u2013870\u00b0C \/ 1555\u20131600\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ucc98\ub9ac \uc804\uc5d0 \uacf5\uad6c\uc758 \ud3c9\ud615\uc744 \ub9de\ucda5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190\u20131230\u00b0C \/ 2175\u20132245\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc778\uc131 \ubc94\uc704\ub294 \ub0ae\uace0, \uacbd\ub3c4, \ub0b4\ub9c8\ubaa8\uc131 \ubc0f \ub0b4\uc5f4\uacbd\ub3c4 \ubc94\uc704\ub294 \ub192\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uadf8\ub294 \uc2dc\uac04<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc77c\ubc18\uc801\uc73c\ub85c \ud3c9\ud615 \uc0c1\ud0dc \ud6c4 2~5\ubd84<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc7a5\uc2dc\uac04 \ub2f4\uac00\ub450\uc9c0 \ub9c8\uc138\uc694.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c, \uacf5\uae30 \ub610\ub294 \uc18c\uae08\ubb3c \ubaa9\uc695<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 66~93\u00b0C(150~200\u00b0F)\uae4c\uc9c0 \uae09\ub7ad\ud558\uc2ed\uc2dc\uc624.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \uc0c1\ud0dc \uacbd\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 64~66 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc989\uc2dc \uc5f4\ucc98\ub9ac\ud558\uc2ed\uc2dc\uc624. M2\ub97c \ub2f4\uae08\uc9c8\ud55c \uc0c1\ud0dc \uadf8\ub300\ub85c \ub450\uc9c0 \ub9c8\uc2ed\uc2dc\uc624.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc120\ud0dd \uc0ac\ud56d\uc778 \uc601\ud558 \uc628\ub3c4 \ucc98\ub9ac<\/td><td class=\"has-text-align-left\" data-align=\"left\">-100~-195\u00b0C \/ -150~-320\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uce58\uc218 \uc548\uc815\uc131\uc774 \ub9e4\uc6b0 \uc911\uc694\ud55c \uacbd\uc6b0\uc5d0 \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub728\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">538\u2013595\u00b0C \/ 1000\u20131105\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc774\uc911 \uc5f4\ucc98\ub9ac\uac00 \ud544\uc218\uc801\uc785\ub2c8\ub2e4. \uc0bc\uc911 \uc5f4\ucc98\ub9ac\ub294 \uae4c\ub2e4\ub85c\uc6b4 \uacf5\uad6c\uc5d0 \uc790\uc8fc \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc77c\ubc18\uc801\uc778 \ucd5c\uc885 \uacbd\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 60~65 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4, \ub2f4\uae08\uc9c8 \ubc29\ubc95, \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \ub2e8\uba74 \ud06c\uae30\uc5d0 \ub530\ub77c \ub2e4\ub985\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">M2\ub294 \uac00\ub2a5\ud558\uba74 \uc9c4\uacf5\ub85c, \uc81c\uc5b4\ub41c \uc911\uc131 \ubd84\uc704\uae30 \ub610\ub294 \uc911\uc131 \uc5fc\uc695\uc5d0\uc11c \uac00\uc5f4\ud574\uc57c \ud569\ub2c8\ub2e4. M2 \uacbd\ud654 \uc628\ub3c4\uc5d0\uc11c \ud45c\uba74 \ud0c8\ud0c4\uc774 \ubc1c\uc0dd\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc774\ub85c \uc778\ud574 \uc678\ubd80\uce35\uc774 \uc5f0\ud654\ub418\uc5b4 \ub0b4\ub9c8\ubaa8\uc131\uc774 \uc800\ud558\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">M2 \uacf5\uad6c\uac15 \uc5f4\ucc98\ub9ac \ubc29\ubc95 (\ub2e8\uacc4\ubcc4)<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \uc5f4\ucc98\ub9ac\ub294 \uc5f0\uc18d\uc801\uc778 \uc57c\uae08 \uacf5\uc815\uc73c\ub85c \uad00\ub9ac\ub418\uc5b4\uc57c \ud558\uba70, \uac01 \ub2e8\uacc4\ub294 \uc11c\ub85c \uc5f0\uad00\ub418\uc5b4 \uc601\ud5a5\uc744 \ubbf8\uce69\ub2c8\ub2e4. \ubd88\ucda9\ubd84\ud55c \uc608\uc5f4\uc740 \uc5f4\ucda9\uaca9\uacfc \uade0\uc5f4 \ubc1c\uc0dd \uac00\ub2a5\uc131\uc744 \ub192\uc785\ub2c8\ub2e4. \ucd5c\uc801\ud654\ub418\uc9c0 \uc54a\uc740 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ub294 \ud0c4\ud654\ubb3c \uc6a9\ud574\ub97c \ubc29\ud574\ud558\uace0 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ub97c \uc99d\uac00\uc2dc\ud0b5\ub2c8\ub2e4. \ubd80\uc801\uc808\ud55c \ub2f4\uae08\uc9c8\uc740 \ub2ec\uc131 \uac00\ub2a5\ud55c \uacbd\ub3c4\ub97c \uc800\ud558\uc2dc\ud0a4\uace0 \ubcc0\ud615\uc744 \uc720\ubc1c\ud569\ub2c8\ub2e4. \ubd88\ucda9\ubd84\ud55c \ub2e4\ub2e8\uacc4 \ud15c\ud37c\ub9c1\uc740 \ubbf8\uc138\uad6c\uc870\ub97c \ubd88\uc548\uc815\ud55c \uc0c1\ud0dc\ub85c \ub9cc\ub4ed\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">1\ub2e8\uacc4: \uacbd\ud654 \uc804 \uc751\ub825 \uc644\ud654<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \uacf5\uad6c\ub97c \uacbd\ud654 \uc804\uc5d0 \uacfc\ub3c4\ud558\uac8c \uac00\uacf5\ud55c \uacbd\uc6b0 \uc751\ub825 \uc81c\uac70 \ucc98\ub9ac\ub97c \uad8c\uc7a5\ud569\ub2c8\ub2e4. \uc7ac\ub8cc\uac00 \ub9ce\uc774 \uc81c\uac70\ub418\uba74 \ub0b4\ubd80 \uac00\uacf5 \uc751\ub825\uc73c\ub85c \uc778\ud574 \ucd5c\uc885 \uc5f4\ucc98\ub9ac \uacfc\uc815\uc5d0\uc11c \ubcc0\ud615\uc774\ub098 \uade0\uc5f4\uc774 \ubc1c\uc0dd\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uacf5\uad6c\ub97c 650~675\u00b0C(1200~1245\u00b0F)\uae4c\uc9c0 \ucc9c\ucc9c\ud788 \uac00\uc5f4\ud558\uace0 \ub2e8\uba74\uc801 1\uc778\uce58\ub2f9 \uc57d 1~2\uc2dc\uac04 \ub3d9\uc548 \uc720\uc9c0\ud569\ub2c8\ub2e4. \uacf5\uad6c\ub97c \uc2e4\uc628\uae4c\uc9c0 \ucc9c\ucc9c\ud788 \ub0c9\uac01\ud569\ub2c8\ub2e4. \uc774 \ub2e8\uacc4\ub294 \uac15\uc7ac\ub97c \uacbd\ud654\uc2dc\ud0a4\ub294 \uac83\uc774 \uc544\ub2c8\ub77c \uace0\uc628 \uacbd\ud654 \uacf5\uc815 \uc804\uc5d0 \ub0b4\ubd80 \uc751\ub825\uc744 \ud574\uc18c\ud558\ub294 \uac83\uc785\ub2c8\ub2e4. \uc751\ub825 \ud574\uc18c \uc804\uc5d0 \ud669\uc0ad \uac00\uacf5\uc744 \uc644\ub8cc\ud558\uc2ed\uc2dc\uc624. \uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1 \ud6c4 \ucd5c\uc885 \uc5f0\uc0ad\uc744 \uc704\ud55c \ucda9\ubd84\ud55c \uc5ec\uc720\ub97c \ub0a8\uaca8 \ub450\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">2\ub2e8\uacc4: M2 \uacf5\uad6c\uac15\uc758 \uc774\uc911 \uc608\uc5f4<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">M2\ub294 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc601\uc5ed\uc5d0 \uc9c1\uc811 \ub123\uc5b4\uc11c\ub294 \uc548 \ub429\ub2c8\ub2e4. \ud569\uae08 \ud568\ub7c9\uc774 \ub192\uace0 \uacbd\ud654 \uc628\ub3c4\uac00 \ub192\uae30 \ub54c\ubb38\uc5d0 \uace0\uc628\uc5d0 \uc9c1\uc811 \uac00\uc5f4\ud558\uba74 \uc2ec\uac01\ud55c \uc5f4\ucda9\uaca9\uc774 \ubc1c\uc0dd\ud558\uc5ec \uade0\uc5f4 \uc704\ud5d8\uc774 \uc99d\uac00\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc608\uc5f4 \ub2e8\uacc4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc628\ub3c4 \ubc94\uc704<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubaa9\uc801<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uccab \ubc88\uc9f8 \uc608\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">540~650\u00b0C \/ 1000~1200\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucd08\uae30 \uc628\ub3c4 \ucda9\uaca9\uc744 \uc904\uc774\uace0 \uade0\uc77c\ud55c \uac00\uc5f4\uc744 \uc2dc\uc791\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub450 \ubc88\uc9f8 \uc608\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">845\u2013870\u00b0C \/ 1555\u20131600\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uae09\uc18d \uac00\uc5f4\ud558\uc5ec \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ubc94\uc704\uc5d0 \ub3c4\ub2ec\ud558\uae30 \uc804\uc5d0 \uacf5\uad6c\uc758 \uc628\ub3c4\ub97c \uade0\uc77c\ud558\uac8c \uc870\uc815\ud569\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\uc608\uc5f4\uc758 \ubaa9\uc801\uc740 \uc628\ub3c4\ub97c \uade0\uc77c\ud558\uac8c \ud558\ub294 \uac83\uc774\uc9c0 \uc7a5\uc2dc\uac04 \uc720\uc9c0\ud558\ub294 \uac83\uc774 \uc544\ub2d9\ub2c8\ub2e4. \uade0\uc77c\ud558\uac8c \uac00\uc5f4\ub418\uba74 \uc9c0\uccb4 \uc5c6\uc774 \uacf5\uad6c\ub97c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ud558\uc2ed\uc2dc\uc624. \uac00\uc5f4 \uc911 \uacfc\ub3c4\ud55c \uc720\uc9c0\ub294 \ubd88\ud544\uc694\ud558\uba70, \ud2b9\ud788 \ubd84\uc704\uae30 \ubcf4\ud638\uac00 \uc81c\ub300\ub85c \ub418\uc9c0 \uc54a\uc740 \uacbd\uc6b0 \ud0c8\ud0c4\uc774 \uc99d\uac00\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc77c\ubd80 \ucc38\uace0 \ubb38\ud5cc\uc5d0\uc11c\ub294 \uc77c\ubc18\uc801\uc778 M2 \uc608\uc5f4 \ubc94\uc704\ub97c 730~845\u00b0C\ub85c \uc81c\uc2dc\ud558\uac70\ub098, 843\u00b0C\uc640 1010\u00b0C\uc758 \uace0\uc628 2\ub2e8\uacc4 \uc0ac\uc774\ud074\uc744 \uc81c\uc2dc\ud569\ub2c8\ub2e4. \uba85\ud655\ud558\uace0 \ub2e8\uacc4\uc801\uc778 \uacf5\uc815\uc744 \uc704\ud574\uc11c\ub294 540~650\u00b0C\uc640 845~870\u00b0C \uc21c\uc11c\uac00 \uc774\ud574\ud558\uae30 \uc27d\uace0 \uacbd\ud654 \uc804 \uac00\uc5f4 \uc21c\uc11c\ub97c \uc9c1\uc811\uc801\uc73c\ub85c \uc124\uba85\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">3\ub2e8\uacc4: \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4 \ubc0f \uc720\uc9c0 \uc2dc\uac04<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">M2\ub294 \uc77c\ubc18\uc801\uc73c\ub85c 1190~1230\u00b0C(2175~2245\u00b0F)\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ub429\ub2c8\ub2e4. \uc774 \ub2e8\uacc4\uac00 \uac00\uc7a5 \uc911\uc694\ud569\ub2c8\ub2e4. \uc628\ub3c4\ub294 \ud544\uc694\ud55c \ud569\uae08 \ud0c4\ud654\ubb3c\uc744 \uc6a9\ud574\uc2dc\ud0a4\uae30\uc5d0 \ucda9\ubd84\ud574\uc57c \ud558\uc9c0\ub9cc, \uacb0\uc815\ub9bd \uc870\ub300\ud654, \uacfc\ub3c4\ud55c \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \ub610\ub294 \uc5f4 \uc190\uc0c1\uc774 \ubc1c\uc0dd\ud558\ub294 \uc784\uacc4\uac12 \ubbf8\ub9cc\uc774\uc5b4\uc57c \ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ud0c0\uac9f<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc628\ub3c4 \ubc94\uc704<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc751\uc6a9 \ub85c\uc9c1<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uac15\uc778\ud568 \uc6b0\uc120 \uc21c\uc704<\/td><td class=\"has-text-align-left\" data-align=\"left\">1175\u20131190\u00b0C \/ 2150\u20132175\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \uacbd\ub3c4\ubcf4\ub2e4 \uc778\uc131\uacfc \uade0\uc5f4 \uc800\ud56d\uc131\uc774 \ub354 \uc911\uc694\ud560 \ub54c \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud45c\uc900 M2 \uacbd\ud654 \ubc94\uc704<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190\u20131230\u00b0C \/ 2175\u20132245\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">M2 \uc808\uc0ad \uacf5\uad6c \ubc0f \ub0b4\ub9c8\ubaa8\uc131 \uacf5\uad6c\uc758 \uc77c\ubc18\uc801\uc778 \ubc94\uc704\uc785\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \uacbd\ub3c4 \ubc0f \ub0b4\ub9c8\ubaa8\uc131<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 1230\u00b0C \/ 2245\u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub192\uc740 \uacbd\ub3c4, \ub0b4\ub9c8\ubaa8\uc131 \ubc0f \ub0b4\uc5f4\uacbd\ub3c4\uac00 \uc694\uad6c\ub418\ub294 \uacbd\uc6b0\uc5d0 \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc18c\uae08\uc695 \uc870\uc808<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 14\u00b0C \/ 25\u00b0F \uc815\ub3c4 \ub0ae\uc544\uc9d1\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5fc\uc695 \ud6c4 \uacbd\ud654 \uacfc\uc815\uc5d0\uc11c \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uace0\ud0c4\uc18c M2 \uc870\uc808<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 14\u00b0C \/ 25\u00b0F \uc815\ub3c4 \ub0ae\uc544\uc9d1\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacfc\uc5f4 \ubc0f \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \uc704\ud5d8\uc744 \uc904\uc774\ub294 \ub370 \ub3c4\uc6c0\uc774 \ub429\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\uc624\uc2a4\ud14c\ub098\uc774\uc9d5 \uc628\ub3c4\uc5d0\uc11c\uc758 \uc720\uc9c0 \uc2dc\uac04\uc740 \uc9e7\uc544\uc57c \ud569\ub2c8\ub2e4. \uacf5\uad6c\uac00 \uc628\ub3c4\uc5d0 \ub3c4\ub2ec\ud558\uba74 M2 \uacf5\uc815\uc5d0\uc11c \uc57d 2~5\ubd84 \uc815\ub3c4\ub9cc \uc720\uc9c0\ud558\uc2ed\uc2dc\uc624. \uc774 \uc2dc\uac04\uc740 \uc804\uccb4 \uc6a9\uad11\ub85c \uacf5\uc815 \uc2dc\uac04\uc774 \uc544\ub2c8\ub77c, \ub2e8\uba74\uc774 \uade0\uc77c\ud574\uc9c4 \ud6c4 \uc628\ub3c4\ub97c \uc720\uc9c0\ud558\ub294 \uc2dc\uac04\uc785\ub2c8\ub2e4. \uac00\uc5f4 \uc2dc\uac04\uc740 \uc720\uc9c0 \uc2dc\uac04\uc5d0 \ud3ec\ud568\ub418\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \ub9e4\uc6b0 \ud070 \ub2e8\uba74\uc758 \uacbd\uc6b0 \uc57d 5~7\ubd84\uc774 \ud544\uc694\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc800\ud569\uae08\uac15\ucc98\ub7fc M2 \uacf5\uc815\uc744 \uc7a5\uc2dc\uac04 \uc720\uc9c0\ud558\uc9c0 \ub9c8\uc2ed\uc2dc\uc624.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \uc5f4\ucc98\ub9ac \uc2e4\ud328\uc758 \uac00\uc7a5 \ud754\ud55c \uc6d0\uc778 \uc911 \ud558\ub098\ub294 \uace0\uc628 \uc720\uc9c0 \uc2dc\uac04 \ucd08\uacfc\uc785\ub2c8\ub2e4. \uace0\uc628\uc5d0\uc11c \ub108\ubb34 \uc624\ub798 \uc720\uc9c0\ud558\uba74 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc5d0 \ud0c4\uc18c\uc640 \ud569\uae08\uc774 \uacfc\ub3c4\ud558\uac8c \uc6a9\ud574\ub418\uc5b4 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uac00 \uc99d\uac00\ud558\uace0 \uacb0\uc815\ub9bd\uc774 \uc870\ub300\ud654\ub418\uba70 \uc778\uc131\uc774 \uc800\ud558\ub429\ub2c8\ub2e4. \ubc18\ub300\ub85c, \uc800\uc628 \uc720\uc9c0\ub294 \uc815\ubc18\ub300\uc758 \ud6a8\uacfc\ub97c \uac00\uc838\uc635\ub2c8\ub2e4. \ud0c4\ud654\ubb3c \uc6a9\ud574\uac00 \ubd88\ucda9\ubd84\ud574\uc838 \uacbd\ub3c4\uac00 \ub0ae\uc544\uc9c0\uace0 \ud15c\ud37c\ub9c1 \uacfc\uc815\uc5d0\uc11c 2\ucc28 \uacbd\ud654\uac00 \uc57d\ud574\uc9d1\ub2c8\ub2e4. \ub530\ub77c\uc11c \ubaa9\ud45c\ub294 \ucd5c\ub300 \uc720\uc9c0 \uc2dc\uac04\uc774 \uc544\ub2c8\ub77c \uc881\uc740 \ubc94\uc704 \ub0b4\uc5d0\uc11c \uc81c\uc5b4\ub41c \ud0c4\ud654\ubb3c \uc6a9\ud574\ub97c \ub2ec\uc131\ud558\ub294 \uac83\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">4\ub2e8\uacc4: \ub2f4\uae08\uc9c8 \ubc29\ubc95: \uc624\uc77c, \uacf5\uae30, \uc5fc\uc695<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ucc98\ub9ac \ud6c4, M2\ub97c \uc624\uc77c, \uacf5\uae30 \ub610\ub294 \uace0\uc628 \uc5fc\uc695\uc5d0\uc11c \ub2f4\uae08\uc9c8\ud569\ub2c8\ub2e4. \ucd5c\uc801\uc758 \ubc29\ubc95\uc740 \uacf5\uad6c \ud06c\uae30, \ubaa9\ud45c \uacbd\ub3c4, \ubcc0\ud615 \ud5c8\uc6a9 \uc624\ucc28 \ubc0f \uc0ac\uc6a9 \uac00\ub2a5\ud55c \uc7a5\ube44\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \ubc29\ubc95<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucd5c\uc801 \uc0ac\uc6a9<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc8fc\uc694 \uc81c\ud55c \uc0ac\ud56d<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \ub2f4\uae08\uc9c8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub354 \ub192\uc740 \uacbd\ub3c4 \ubc18\uc751<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacf5\ub7ad\uc2dd\ubcf4\ub2e4 \ubcc0\ud615 \ubc0f \uade0\uc5f4 \uc704\ud5d8\uc774 \ub354 \ub192\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uacf5\uae30 \ub2f4\uae08\uc9c8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uce58\uc218 \uc548\uc815\uc131 \ud5a5\uc0c1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4\ub294 \ud06c\uae30\uac00 \ud06c\uac70\ub098 \ub0c9\uac01 \uc18d\ub3c4\uac00 \ub290\ub9b0 \ubd80\ubd84\uc5d0\uc11c \ub354 \ub0ae\uc744 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub728\uac70\uc6b4 \uc18c\uae08\ubb3c \ub2f4\uae08\uc9c8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc6b0\uc218\ud55c \uc628\ub3c4 \uade0\uc77c\ud654 \ubc0f \uc5f4\ucda9\uaca9 \uac10\uc18c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc801\uc808\ud55c \uc5fc\uc695 \uc7a5\ube44\uc640 \uc5c4\uaca9\ud55c \uad00\ub9ac\uac00 \ud544\uc694\ud569\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\uc624\uc77c \ud01c\uce6d\uc740 \ucd5c\ub300 \uacbd\ub3c4 \ubc18\uc751\uc774 \uc694\uad6c\ub420 \ub54c \uc8fc\ub85c \uc120\ud0dd\ub418\uba70, \uacf5\uad6c\ub97c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc0c1\ud0dc\uc5d0\uc11c 66~93\u00b0C(150~200\u00b0F)\uae4c\uc9c0 \ub0c9\uac01\ud569\ub2c8\ub2e4. \uacf5\uae30 \ud01c\uce6d\uc740 \ube44\uad50\uc801 \uc628\ud654\ud558\uace0 \ubcc0\ud615 \uc704\ud5d8\uc744 \uc904\uc5ec\uc8fc\ubbc0\ub85c, \uae09\uaca9\ud55c \ub0c9\uac01\ubcf4\ub2e4\ub294 \uce58\uc218 \uc548\uc815\uc131\uc774 \uc911\uc694\ud55c \uc18c\ud615 \ubd80\ud488\uc774\ub098 \uacf5\uad6c\uc5d0 \uc801\ud569\ud569\ub2c8\ub2e4. \uace0\uc628 \uc5fc\uc695 \ud01c\uce6d\uc740 \uc628\ub3c4 \uade0\uc77c\ud654\ub97c \ub354\uc6b1 \ud6a8\uacfc\uc801\uc73c\ub85c \uc81c\uc5b4\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uacf5\uad6c\uc758 \ub2e8\uba74 \uc628\ub3c4\uac00 \uade0\uc77c\ud574\uc9c8 \ub54c\uae4c\uc9c0 \uc720\uc9c0\ud55c \ud6c4, \ud15c\ud37c\ub9c1 \uc804\uc5d0 \ucd94\uac00\ub85c \ub0c9\uac01\ud558\uc5ec \uc5f4 \ucda9\uaca9\uacfc \ubcc0\ud615\uc744 \ucd5c\uc18c\ud654\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub2f4\uae08\uc9c8 \ub9e4\uccb4\uc640 \uad00\uacc4\uc5c6\uc774 \uacf5\uad6c\uac00 66~93\u00b0C\ub85c \ub0c9\uac01\ub418\ub294 \uc989\uc2dc \ud15c\ud37c\ub9c1\uc744 \uc2dc\uc791\ud574\uc57c \ud569\ub2c8\ub2e4. \ub2f4\uae08\uc9c8 \uc9c1\ud6c4\uc758 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8 \uc0c1\ud0dc\ub97c \uc7a5\uc2dc\uac04 \uc720\uc9c0\ud558\uba74 \ud15c\ud37c\ub9c1\ub418\uc9c0 \uc54a\uc740 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc640 \uc794\ub958 \uc751\ub825\uc73c\ub85c \uc778\ud574 \uc9c0\uc5f0 \uade0\uc5f4\uc774\ub098 \uce58\uc218 \ubcc0\ud615\uc774 \ubc1c\uc0dd\ud560 \uc704\ud5d8\uc774 \ucee4\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/12\/Time-temperature-transformation-diagram-for-M2-high-speed-tool-steel.avif\" alt=\"M2 \uace0\uc18d \uacf5\uad6c\uac15\uc758 \uc2dc\uac04-\uc628\ub3c4-\ubcc0\ud658 \ub2e4\uc774\uc5b4\uadf8\ub7a8\"\/><figcaption class=\"wp-element-caption\"><strong>\uadf8\ub9bc: 1230\u00b0C\/2250\u00b0F\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654\ub41c M2 \uace0\uc18d \uacf5\uad6c\uac15\uc758 \uc0c1\ubcc0\ud654 \ub2e4\uc774\uc5b4\uadf8\ub7a8. \uc5fc\ub0c9, \uacf5\ub0c9 \ubc0f \uacf5\ub0c9 \uace1\uc120\uc774 \uc911\ucca9\ub418\uc5b4 \ud45c\uc2dc\ub428.<\/strong>\n \uc774 \ub3c4\ud45c\ub294 \ud384\ub77c\uc774\ud2b8 \ubc0f \ubca0\uc774\ub098\uc774\ud2b8 \ubcc0\ud0dc \uc601\uc5ed, \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uc758 \uc2dc\uc791 \ubd80\ubd84, \uadf8\ub9ac\uace0 15%, 50%, 90% \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8 \ubcc0\ud0dc\uc120\uc744 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \ucd9c\ucc98: ASM \ud578\ub4dc\ubd81, \uc81c16\uad8c, \uac00\uacf5, 121\ud398\uc774\uc9c0.<\/figcaption><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">5\ub2e8\uacc4: \uc120\ud0dd \uc0ac\ud56d\uc778 \uc601\ud558 \uc628\ub3c4 \ucc98\ub9ac<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\uadf9\uc800\uc628 \ucc98\ub9ac\ub294 \uc120\ud0dd \uc0ac\ud56d\uc785\ub2c8\ub2e4. \uc8fc\ub85c \ubcf5\uc7a1\ud55c \uacf5\uad6c, \uc815\ubc00 \ubd80\ud488 \ub610\ub294 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ub97c \ucd94\uac00\ub85c \uc904\uc5ec\uc57c \ud558\ub294 \ubd80\ud488\uacfc \uac19\uc774 \uce58\uc218 \uc548\uc815\uc131\uc774 \uc911\uc694\ud55c \uacbd\uc6b0\uc5d0 \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc77c\ubc18\uc801\uc778 \uadf9\uc800\uc628 \ubc94\uc704\ub294 -100~-195\u00b0C(-150~-320\u00b0F)\uc785\ub2c8\ub2e4. \ubd80\ud488\uc774 \uc2e4\uc628\uc73c\ub85c \ub3cc\uc544\uc628 \ud6c4\uc5d0\ub294 \uc989\uc2dc \ud15c\ud37c\ub9c1\uc744 \uc2dc\uc791\ud574\uc57c \ud569\ub2c8\ub2e4. \ubcf5\uc7a1\ud55c \ud615\uc0c1\uc758 \uacbd\uc6b0, \uade0\uc5f4 \ubc1c\uc0dd \uc704\ud5d8\uc744 \uc904\uc774\uae30 \uc704\ud574 \ub3d9\uacb0 \uc804\uc5d0 \uc9e7\uc740 \uc2dc\uac04 \ub3d9\uc548 \uc800\uc628 \uc751\ub825 \uc644\ud654 \ud15c\ud37c\ub9c1\uc744 \uc801\uc6a9\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uadf9\uc800\uc628 \ucc98\ub9ac\ub294 \uc801\uc808\ud55c \uc624\uc2a4\ud14c\ub098\uc774\uc9d5, \ub2f4\uae08\uc9c8 \ubc0f \ub2e4\uc911 \ud15c\ud37c\ub9c1\uc744 \ub300\uccb4\ud558\ub294 \uac83\uc774 \uc544\ub2d9\ub2c8\ub2e4. \uc774\ub294 \uacf5\uad6c \uc124\uacc4 \ubc0f \uc0ac\uc6a9 \uc870\uac74\uc5d0 \ub530\ub77c \ud544\uc694\ud55c \uacbd\uc6b0 \ucd94\uac00\uc801\uc778 \uc548\uc815\ud654 \ub2e8\uacc4\uc77c \ubfd0\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">6\ub2e8\uacc4: \uc774\uc911 \ub610\ub294 \uc0bc\uc911 \ub2f4\uae08\uc9c8<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\ub2f4\uae08\uc9c8 \uc9c1\ud6c4 \ud15c\ud37c\ub9c1\uc744 \uc2dc\uc791\ud574\uc57c \ud569\ub2c8\ub2e4. \uc601\ud558 \uc774\ud558\uc758 \uc800\uc628 \uc0ac\uc774\ud074\uc744 \uc0ac\uc6a9\ud558\ub294 \uacbd\uc6b0, \ubd80\ud488\uc774 \uc2e4\uc628\uc73c\ub85c \ub3cc\uc544\uc624\uc790\ub9c8\uc790 \uc989\uc2dc \ud15c\ud37c\ub9c1\uc744 \uc2e4\uc2dc\ud574\uc57c \ud569\ub2c8\ub2e4. M2 \uacf5\ubc95\uc740 2\ucc28 \uacbd\ud654\uc5d0 \uc758\uc874\ud569\ub2c8\ub2e4. \ud15c\ud37c\ub9c1\uc740 \ub2e8\uc21c\ud788 \uc751\ub825\uc744 \uc644\ud654\ud558\ub294 \uac83 \uc774\uc0c1\uc758 \uc5ed\ud560\uc744 \ud569\ub2c8\ub2e4. \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc758 \ubcc0\ud0dc, \ud0c4\ud654\ubb3c \uc11d\ucd9c, \ucd5c\uc885 \uacbd\ub3c4 \ubc0f \uc778\uc131\uc744 \uc81c\uc5b4\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">M2\uac15\uc758 \uc77c\ubc18\uc801\uc778 \ud15c\ud37c\ub9c1 \ubc94\uc704\ub294 538~595\u00b0C(1000~1105\u00b0F)\uc785\ub2c8\ub2e4. \uc774\uc911 \ud15c\ud37c\ub9c1\uc740 \uc2e4\uc9c8\uc801\uc778 \ucd5c\uc18c \uc694\uad6c \uc0ac\ud56d\uc774\uba70, \uc0bc\uc911 \ud15c\ud37c\ub9c1\uc740 \uc808\uc0ad \uacf5\uad6c, \uc815\ubc00 \uacf5\uad6c \ubc0f \uae4c\ub2e4\ub85c\uc6b4 \uc0ac\uc6a9 \ud658\uacbd\uc5d0 \uc790\uc8fc \uc0ac\uc6a9\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uac01 \ud15c\ud37c\ub9c1 \uc0ac\uc774\ud074 \ud6c4\uc5d0\ub294 \ub2e4\uc74c \uc0ac\uc774\ud074\uc744 \uc2dc\uc791\ud558\uae30 \uc804\uc5d0 \uc2e4\uc628\uae4c\uc9c0 \ub0c9\uac01\ud574\uc57c \ud569\ub2c8\ub2e4. \uc774 \ub0c9\uac01 \ub2e8\uacc4\ub294 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uac00 \ub0c9\uac01 \uc911\uc5d0 \uc0c8\ub85c\uc6b4 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\ub85c \ubcc0\ud0dc\ub420 \uc218 \uc788\uace0, \ub2e4\uc74c \ud15c\ud37c\ub9c1\uc5d0\uc11c \uc0c8\ub85c \ud615\uc131\ub41c \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uc758 \uc751\ub825\uc774 \ud574\uc18c\ub418\uae30 \ub54c\ubb38\uc5d0 \uc911\uc694\ud569\ub2c8\ub2e4. M2\uc758 \uacbd\uc6b0 \ub2e8\uc77c \ud15c\ud37c\ub9c1\ub9cc\uc73c\ub85c\ub294 \ucda9\ubd84\ud558\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \uc77c\ubc18\uc801\uc73c\ub85c \ud55c \ubc88\uc758 \uc0ac\uc774\ud074\ub85c\ub294 \uad6c\uc870\ub97c \uc548\uc815\ud654\ud558\uae30\uc5d0 \ucda9\ubd84\ud558\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">M2 \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uacbd\ub3c4\ud45c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">M2\ub294 \uac15\ub825\ud55c 2\ucc28 \uacbd\ud654 \ubc18\uc751\uc744 \ubcf4\uc785\ub2c8\ub2e4. \ud15c\ud37c\ub9c1 \uc628\ub3c4\uac00 \uc0c1\uc2b9\ud568\uc5d0 \ub530\ub77c \uacbd\ub3c4\uac00 \ub2e8\uc21c\ud788 \uac10\uc18c\ud558\ub294 \uac83\uc774 \uc544\ub2c8\ub77c, \uace0\uc628 \ud15c\ud37c\ub9c1 \uc601\uc5ed\uc5d0\uc11c \ubbf8\uc138\ud55c \ud569\uae08 \ud0c4\ud654\ubb3c\uc774 \uc11d\ucd9c\ub418\uc5b4 \uacbd\ub3c4\uac00 \ub2e4\uc2dc \uc0c1\uc2b9\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc544\ub798 \ucc28\ud2b8\ub294 M2 \ud569\uae08\uc744 \uc57d 1230\u00b0C\/2250\u00b0F\uc5d0\uc11c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \ucc98\ub9ac\ud55c \ud6c4 \ub098\ud0c0\ub098\ub294 \uc77c\ubc18\uc801\uc778 \uacbd\ub3c4\ub97c \ubcf4\uc5ec\uc90d\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc624\uc77c \ub2f4\uae08\uc9c8 \uacbd\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacf5\uae30 \ub2f4\uae08\uc9c8 \uacbd\ub3c4<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \uc9c1\ud6c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0\u201366.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0\u201366.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">400\u00b0F \/ 204\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">500\u00b0F \/ 260\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">600\u00b0F \/ 316\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">700\u00b0F \/ 371\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">800\u00b0F \/ 427\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">900\u00b0F \/ 482\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1000\u00b0F \/ 540\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.5\u201365.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1025\u00b0F \/ 550\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">65.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1050\u00b0F \/ 565\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5\u201365.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1100\u00b0F \/ 595\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.5\u201364.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1150\u00b0F \/ 620\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.0\u201362.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1200\u00b0F \/ 650\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.0\u201353.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.0 HRC<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \uc808\uc0ad \ubc0f \uacf5\uad6c \uc751\uc6a9 \ubd84\uc57c\uc758 \uacbd\uc6b0, 540~565\u00b0C \ubd80\uadfc\uc5d0\uc11c \ud15c\ud37c\ub9c1\uc744 \ud558\ub294 \uac83\uc774 \uc77c\ubc18\uc801\uc785\ub2c8\ub2e4. \uc774\ub294 2\ucc28 \uacbd\ud654 \ubc94\uc704\uc5d0 \uac00\uae5d\uace0 \uacbd\ub3c4, \uc808\uc0ad \uc131\ub2a5, \uc778\uc131 \ubc0f \uc548\uc815\uc131\uc758 \uade0\ud615\uc744 \uc774\ub8e8\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \ud569\uae08\uc740 \ud15c\ud37c\ub9c1 \uc628\ub3c4\uac00 \ub108\ubb34 \ub0ae\uac70\ub098 \ud15c\ud37c\ub9c1 \ud69f\uc218\uac00 \ubd80\uc871\ud558\uba74 \ub0b4\ubd80 \uc751\ub825\uc774 \ub192\uc544\uc9c0\uace0 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uac00 \ubd88\uc548\uc815\ud574\uc9c8 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ucd5c\uc18c 2\ud68c \ud15c\ud37c\ub9c1\uc774 \ud544\uc694\ud558\uba70, \ub354\uc6b1 \uae4c\ub2e4\ub85c\uc6b4 \uacf5\uad6c\uc5d0\ub294 3\ud68c \ud15c\ud37c\ub9c1\uc774 \uc0ac\uc6a9\ub418\ub294 \uacbd\uc6b0\uac00 \ub9ce\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4\uac00 M2 \ud15c\ud37c\ub9c1 \uacbd\ub3c4\uc5d0 \ubbf8\uce58\ub294 \uc601\ud5a5<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4\ub294 \ucd5c\uc885 \uacbd\ub3c4\uc5d0 \uc601\ud5a5\uc744 \ubbf8\uce69\ub2c8\ub2e4. \uacbd\ud654 \uc628\ub3c4\uac00 \ub192\uc744\uc218\ub85d \ub354 \ub9ce\uc740 \ud0c4\uc18c\uc640 \ud569\uae08 \uc6d0\uc18c\uac00 \uc6a9\ud574\ub418\uc5b4 \ud15c\ud37c\ub9c1 \uc911 2\ucc28 \uacbd\ud654\uac00 \uac15\ud654\ub418\uc9c0\ub9cc, \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8 \ud568\ub7c9\uc774 \uc99d\uac00\ud558\uace0 \uacfc\uc5f4 \uc704\ud5d8\ub3c4 \ucee4\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc544\ub798 \ud45c\ub294 \u00b0C \ub2e8\uc704\ub85c \ubcf4\uace0\ub41c \ubcc4\ub3c4\uc758 \ub370\uc774\ud130 \uc138\ud2b8\ub97c \uc0ac\uc6a9\ud558\ubbc0\ub85c \ucd5c\uace0\uac12\uc774 \uc704\uc758 \u00b0F \uc774\uc911 \ud15c\ud37c\ub9c1 \ucc28\ud2b8\uc640 \uc57d\uac04 \ub2e4\ub985\ub2c8\ub2e4. \ub450 \uacb0\uacfc\ub294 \uc11c\ub85c \ubaa8\uc21c\ub418\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \uc11c\ub85c \ub2e4\ub978 \ubc30\uce58, \uc624\uc2a4\ud14c\ub098\uc774\uc9d5 \uc870\uac74 \ubc0f \uc2dc\ud5d8 \uc124\uc815\uc5d0\uc11c \uc5bb\uc740 \ub370\uc774\ud130\uc774\uba70, \ub458 \ub2e4 \ub3d9\uc77c\ud55c \uacbd\ud5a5\uc744 \ubcf4\uc785\ub2c8\ub2e4. \uc989, 525~550\u00b0C \ubd80\uadfc\uc5d0\uc11c 2\ucc28 \uacbd\ud654 \ucd5c\uace0\uc810\uc774 \ub098\ud0c0\ub09c \ud6c4 575\u00b0C \uc774\uc0c1\uc5d0\uc11c \uac10\uc18c\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4<\/th><th class=\"has-text-align-left\" data-align=\"left\">1180\u00b0C\uc5d0\uc11c \uacbd\ud654\ub428<\/th><th class=\"has-text-align-left\" data-align=\"left\">1200\u00b0C\uc5d0\uc11c \uacbd\ud654<\/th><th class=\"has-text-align-left\" data-align=\"left\">1220\u00b0C\uc5d0\uc11c \uacbd\ud654\ub428<\/th><th class=\"has-text-align-left\" data-align=\"left\">1240\u00b0C\uc5d0\uc11c \uacbd\ud654\ub428<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \uc9c1\ud6c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">66.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">65.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">200\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.5 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">300\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.7 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.5 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">400\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">500\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.5 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">525\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">65.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">65.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">66.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">550\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">65.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">66.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">66.5 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">575\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">64.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">66.0 HRC<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">600\u00b0C<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.5 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0 HRC<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774\ub7ec\ud55c \uc774\uc720\ub85c M2\ub294 \ub2e8\uc21c\ud788 \ucd5c\uace0 \uacbd\ub3c4 \uc218\uce58\ub97c \uc5bb\uae30 \uc704\ud574 \uc5f4\ucc98\ub9ac\ud574\uc11c\ub294 \uc548 \ub429\ub2c8\ub2e4. \uacbd\ud654 \uc628\ub3c4\uac00 \ub192\uc744\uc218\ub85d 2\ucc28 \uacbd\ud654\uac00 \uac15\ud574\uc9c0\uc9c0\ub9cc, \uc548\uc804\ud55c \uac00\uacf5 \uc5ec\uc720\uac00 \uc904\uc5b4\ub4ed\ub2c8\ub2e4. \uc0dd\uc0b0 \ud604\uc7a5\uc5d0\uc11c\ub294 \uc801\uc808\ud55c \uc778\uc131, \uc81c\uc5b4\ub41c \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8, \uadf8\ub9ac\uace0 \uc548\uc815\uc801\uc778 \uacf5\uad6c \uc218\uba85\uc744 \uac16\ucd98 \uc548\uc815\uc801\uc778 \uacbd\ub3c4\ub97c \ubaa9\ud45c\ub85c \ud558\ub294 \uac83\uc774 \ub354 \ubc14\ub78c\uc9c1\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">M2 \uc5f4\ucc98\ub9ac \ubb38\uc81c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \uc5f4\ucc98\ub9ac \uc2e4\ud328\uc758 \ub300\ubd80\ubd84\uc740 \ub2e4\uc74c \ub2e4\uc12f \uac00\uc9c0 \uc601\uc5ed\uc5d0\uc11c \ubc1c\uc0dd\ud569\ub2c8\ub2e4. \uc798\ubabb\ub41c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654, \uacfc\ub3c4\ud55c \uce68\uc9c0 \uc2dc\uac04, \ubd80\uc801\uc808\ud55c \ubd84\uc704\uae30 \ubcf4\ud638, \ubd80\uc801\uc808\ud55c \ub2f4\uae08\uc9c8 \ubc0f \ubd88\ucda9\ubd84\ud55c \ud15c\ud37c\ub9c1.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ubb38\uc81c<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc8fc\uc694 \uc6d0\uc778<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacb0\uacfc<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub0ae\uc740 \uacbd\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacfc\uc18c \uac00\uc5f4, \ubd88\ucda9\ubd84\ud55c \ud0c4\ud654\ubb3c \uc6a9\ud574, \ubd88\ub7c9\ud55c \ub2f4\uae08\uc9c8 \ub610\ub294 \uacfc\ub3c4\ud55c \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud574\ub2f9 \uacf5\uad6c\ub294 \uc694\uad6c\ub418\ub294 \uc791\uc5c5 \uacbd\ub3c4\uc5d0 \ub3c4\ub2ec\ud560 \uc218 \uc5c6\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uacb0\uc815\ub9bd \uc870\ub300\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacfc\uc5f4 \ub610\ub294 \uacfc\ub3c4\ud55c \uce68\uc218<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc778\uc131\uc774 \ub0ae\uace0 \uade0\uc5f4 \uc704\ud5d8\uc774 \ub192\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uacfc\uc789 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub192\uc740 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ud654 \uc628\ub3c4, \uc7a5\uc2dc\uac04 \uc720\uc9c0 \ub610\ub294 \ubd88\ucda9\ubd84\ud55c \ud15c\ud37c\ub9c1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uce58\uc218 \ubcc0\ud654 \ubc0f \ubd88\uc548\uc815\ud55c \uacbd\ub3c4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2f4\uae08\uc9c8 \uade0\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f4\ucda9\uaca9, \uc2ec\ud55c \ub2f4\uae08\uc9c8 \uc751\ub825 \ub610\ub294 \uc9c0\uc5f0\ub41c \ud15c\ud37c\ub9c1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\ud654 \uc911 \ub610\ub294 \uacbd\ud654 \ud6c4\uc5d0 \ubc1c\uc0dd\ud558\ub294 \uade0\uc5f4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud0c8\ud0c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub300\uae30 \ubcf4\ud638 \uc7a5\uce58 \uc5c6\uc774 \uac00\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud45c\uba74\uc774 \ubd80\ub4dc\ub7fd\uace0 \ub0b4\ub9c8\ubaa8\uc131\uc774 \ub5a8\uc5b4\uc9d1\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc628\ub3c4 \uc870\uc808 \ubd80\uc871<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud15c\ud37c\ub9c1 \uc628\ub3c4\uac00 \ub108\ubb34 \ub0ae\uac70\ub098 \ud15c\ud37c\ub9c1 \ud69f\uc218\uac00 \ub108\ubb34 \uc801\uc2b5\ub2c8\ub2e4.<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucde8\uc131 \ubc0f \ubd88\uc548\uc815\ud55c \uad6c\uc870.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">M2\ub294 \uace0\uc628 \ud55c\uacc4\uc5d0 \uac00\uae4c\uc6b4 \uc628\ub3c4\uc5d0\uc11c \uac00\uacf5\ub418\uae30 \ub54c\ubb38\uc5d0 \uacfc\uc5f4 \ubc0f \uacfc\uc18c\ube44\ub294 \uc2ec\uac01\ud55c \ubb38\uc81c\uc785\ub2c8\ub2e4. \uacfc\ub3c4\ud55c \uc628\ub3c4\ub098 \uc2dc\uac04\uc740 \uacb0\uc815\ub9bd\uc744 \uc870\ub300\ud654\ud558\uace0 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ub97c \uc99d\uac00\uc2dc\ud0a4\uba70 \uc778\uc131\uc744 \uc800\ud558\uc2dc\ud0a4\uace0 \uacf5\uad6c\uc758 \uc2e0\ub8b0\uc131\uc744 \ub5a8\uc5b4\ub728\ub9bd\ub2c8\ub2e4. \ubc18\ub300\ub85c \uacfc\uc18c\uc5f4\uc740 \ud569\uae08 \ud0c4\ud654\ubb3c\uc758 \uc6a9\ud574\ub97c \uc800\ud574\ud558\uc5ec \ub2f4\uae08\uc9c8 \uacbd\ub3c4\ub97c \ub0ae\ucd94\uace0 \ud15c\ud37c\ub9c1 \uc911 2\ucc28 \uacbd\ud654\ub97c \uc57d\ud654\uc2dc\ud0b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">M2 \ud569\uae08\uc5d0\uc11c\ub294 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uac00 \uc608\uc0c1\ub418\ub294 \ud604\uc0c1\uc774\uc9c0\ub9cc, \uacfc\ub3c4\ud55c \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ub294 \ubb38\uc81c\ub97c \uc77c\uc73c\ud0b5\ub2c8\ub2e4. \uc0ac\uc6a9 \uc911\uc5d0 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uac00 \ubcc0\ud0dc\ub418\uc5b4 \uc0c8\ub85c\uc6b4 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\ub97c \ud615\uc131\ud558\uace0, \uc774\ub85c \uc778\ud574 \uce58\uc218 \uc99d\uac00 \ubc0f \ub0b4\ubd80 \uc751\ub825\uc774 \ubc1c\uc0dd\ud558\uc5ec \uade0\uc5f4 \uc704\ud5d8\uc774 \ub192\uc544\uc9c8 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ud0c8\ud0c4 \ub610\ud55c \uc8fc\uc694 \ud30c\uc190 \uc6d0\uc778 \uc911 \ud558\ub098\uc785\ub2c8\ub2e4. \uc9c4\uacf5 \uc0c1\ud0dc\uac00 \uc544\ub2cc \uc911\uc131 \ubd84\uc704\uae30\uc5d0\uc11c \ub610\ub294 \uc5fc\uc695 \ubcf4\ud638 \uc5c6\uc774 \uac00\uc5f4\ud560 \uacbd\uc6b0, \ud45c\uba74\uc5d0\uc11c \ud0c4\uc18c\uac00 \uc190\uc2e4\ub418\uc5b4 \uacbd\ud654 \ud6c4\uc5d0\ub3c4 \ud45c\uba74\uc774 \ubb34\ub978 \uc0c1\ud0dc\ub85c \ub0a8\uac8c \ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud15c\ud37c\ub9c1 \uc624\ub958\ub294 \ud2b9\ud788 \ube44\uc6a9\uc774 \ub9ce\uc774 \ub4ed\ub2c8\ub2e4. M2\ub294 \uc794\ub958 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc758 \ubcc0\ud0dc\uc640 \uc0c8\ub85c\uc6b4 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uc758 \ud15c\ud37c\ub9c1\uc774 \ud55c \ubc88\uc758 \ud15c\ud37c\ub9c1 \uc8fc\uae30 \ub0b4\uc5d0 \uc644\ub8cc\ub420 \uc218 \uc5c6\uae30 \ub54c\ubb38\uc5d0 \uc5ec\ub7ec \ubc88\uc758 \ud15c\ud37c\ub9c1 \uc8fc\uae30\uac00 \ud544\uc694\ud569\ub2c8\ub2e4. \uc548\uc815\uc801\uc778 \uc131\ub2a5\uc744 \uc704\ud574\uc11c\ub294 \uac01 \ud15c\ud37c\ub9c1 \uc8fc\uae30 \uc0ac\uc774\uc5d0 \uacf5\uad6c\ub97c \uc2e4\uc628\uc73c\ub85c \ub0c9\uac01\ud574\uc57c \ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Aobo Steel supplies M2 \/ DIN 1.3343 \/ JIS SKH51 high-speed tool steel in the annealed condition and does not provide final heat-treatment services such as hardening, quenching, sub-zero treatment, or tempering.\n The heat-treatment parameters, hardness data, and process recommendations in this guide are provided as general technical support references for customers. Actual results may vary with furnace capability, section size, tool geometry, steel condition, quenching practice, atmosphere control, and final application. Final heat-treatment procedures should be confirmed and validated by the customer\u2019s heat-treatment provider before production.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-7da068b4 wp-block-group-is-layout-constrained\" style=\"border-radius:10px;background-color:#e6f0ff;margin-bottom:0;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<h2 class=\"wp-block-heading\">\ub300\ub7c9 \uc8fc\ubb38\uc5d0 \ud544\uc694\ud55c \uc5b4\ub2d0\ub9c1 \ucc98\ub9ac\ub41c M2 \uace0\uc18d \uacf5\uad6c\uac15\uc744 \ucc3e\uace0 \uacc4\uc2ed\ub2c8\uae4c?<\/h2>\n\n<p class=\"wp-block-paragraph\">\uc544\uc624\ubcf4 \uc2a4\ud2f8\uc740 M2 \/ DIN 1.3343 \/ JIS SKH51 \uaddc\uaca9\uc758 \uc6d0\ud615 \ubd09\uac15 \ubc0f \ud310\uc7ac\ub97c \uacf5\uae09\ud558\uba70, \ucd9c\ud558 \uc804 \uacf5\uc7a5 \uc778\uc99d\uc11c \ubc0f \uce58\uc218 \uac80\uc0ac\ub97c \uc2e4\uc2dc\ud569\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button popmake-16052\"><a class=\"wp-block-button__link wp-element-button\">\ubb38\uc758 \ubcf4\ub0b4\uae30<\/a><\/div>\n\n\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/ko\/m2-tool-steel\/\">M2 \uacf5\uae09 \uc0c1\uc138 \uc815\ubcf4\ub97c \ud655\uc778\ud558\uc138\uc694<\/a><\/div>\n\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>M2 Tool Steel Heat Treatment Guide M2 tool steel is heat-treated by double preheating, austenitizing at 1190\u20131230\u00b0C, quenching in oil, air, or a salt bath, then double or triple tempering at 538\u2013595\u00b0C. Tempered correctly, M2 reaches about 60\u201365 HRC, with the high hardness, wear resistance, and red hardness expected from a high-speed steel. Hardness values [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":15110,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"disabled","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":"[]"},"class_list":["post-11688","page","type-page","status-publish","has-post-thumbnail","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.7 (Yoast SEO v28.7) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>M2 Steel Heat Treatment: Hardening, Tempering &amp; 60\u201365 HRC Chart<\/title>\n<meta name=\"description\" content=\"M2 heat treatment guide with preheating, austenitizing, quenching, tempering temperatures, and hardness chart. Learn how M2 reaches about 60\u201365 HRC.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/m2-tool-steel-heat-treatment\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"M2 Steel Heat Treatment: Hardening, Tempering &amp; 60\u201365 HRC Chart\" \/>\n<meta property=\"og:description\" content=\"M2 heat treatment guide with preheating, austenitizing, quenching, tempering temperatures, and hardness chart. Learn how M2 reaches about 60\u201365 HRC.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/m2-tool-steel-heat-treatment\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-16T00:38:22+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif\" \/>\n\t<meta property=\"og:image:width\" content=\"1254\" \/>\n\t<meta property=\"og:image:height\" content=\"1254\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"13\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"M2 Steel Heat Treatment: Hardening, Tempering &amp; 60\u201365 HRC Chart\",\"datePublished\":\"2025-12-23T06:12:35+00:00\",\"dateModified\":\"2026-10-16T00:38:22+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/\"},\"wordCount\":2221,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/M2-heat-treatment-ad.avif\",\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/\",\"name\":\"M2 Steel Heat Treatment: Hardening, Tempering &amp; 60\u201365 HRC Chart\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/M2-heat-treatment-ad.avif\",\"datePublished\":\"2025-12-23T06:12:35+00:00\",\"dateModified\":\"2026-10-16T00:38:22+00:00\",\"description\":\"M2 heat treatment guide with preheating, austenitizing, quenching, tempering temperatures, and hardness chart. Learn how M2 reaches about 60\u201365 HRC.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/M2-heat-treatment-ad.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/05\\\/M2-heat-treatment-ad.avif\",\"width\":1254,\"height\":1254},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/m2-tool-steel-heat-treatment\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"M2 Steel Heat Treatment: Hardening, Tempering &amp; 60\u201365 HRC Chart\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"M2\uac15 \uc5f4\ucc98\ub9ac: \uacbd\ud654, \ud15c\ud37c\ub9c1 \ubc0f 60~65 HRC \uacbd\ub3c4\ud45c","description":"M2 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc: \uc608\uc5f4, \uc624\uc2a4\ud14c\ub098\uc774\uc9d5, \ub2f4\uae08\uc9c8, \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uacbd\ub3c4\ud45c\ub97c \ud655\uc778\ud558\uc138\uc694. M2\uac00 \uc57d 60~65 HRC\uc758 \uacbd\ub3c4\ub97c \ub2ec\uc131\ud558\ub294 \ubc29\ubc95\uc744 \uc54c\uc544\ubcf4\uc138\uc694.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/m2-tool-steel-heat-treatment\/","og_locale":"ko_KR","og_type":"article","og_title":"M2 Steel Heat Treatment: Hardening, Tempering &amp; 60\u201365 HRC Chart","og_description":"M2 heat treatment guide with preheating, austenitizing, quenching, tempering temperatures, and hardness chart. Learn how M2 reaches about 60\u201365 HRC.","og_url":"https:\/\/aobosteel.com\/ko\/m2-tool-steel-heat-treatment\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-16T00:38:22+00:00","og_image":[{"width":1254,"height":1254,"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif","type":"image\/png"}],"twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"13\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"M2 Steel Heat Treatment: Hardening, Tempering &amp; 60\u201365 HRC Chart","datePublished":"2025-12-23T06:12:35+00:00","dateModified":"2026-10-16T00:38:22+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/"},"wordCount":2221,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif","inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/","url":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/","name":"M2\uac15 \uc5f4\ucc98\ub9ac: \uacbd\ud654, \ud15c\ud37c\ub9c1 \ubc0f 60~65 HRC \uacbd\ub3c4\ud45c","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif","datePublished":"2025-12-23T06:12:35+00:00","dateModified":"2026-10-16T00:38:22+00:00","description":"M2 \uc5f4\ucc98\ub9ac \uac00\uc774\ub4dc: \uc608\uc5f4, \uc624\uc2a4\ud14c\ub098\uc774\uc9d5, \ub2f4\uae08\uc9c8, \ud15c\ud37c\ub9c1 \uc628\ub3c4 \ubc0f \uacbd\ub3c4\ud45c\ub97c \ud655\uc778\ud558\uc138\uc694. M2\uac00 \uc57d 60~65 HRC\uc758 \uacbd\ub3c4\ub97c \ub2ec\uc131\ud558\ub294 \ubc29\ubc95\uc744 \uc54c\uc544\ubcf4\uc138\uc694.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/"]}]},{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif","width":1254,"height":1254},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/m2-tool-steel-heat-treatment\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"M2 Steel Heat Treatment: Hardening, Tempering &amp; 60\u201365 HRC Chart"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif",1254,1254,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-150x150.avif",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-300x300.avif",300,300,true],"medium_large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-768x768.avif",768,768,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-1024x1024.avif",1024,1024,true],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif",1254,1254,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif",1254,1254,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-12x12.avif",12,12,true]},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"M2 Tool Steel Heat Treatment Guide M2 tool steel is heat-treated by double preheating, austenitizing at 1190\u20131230\u00b0C, quenching in oil, air, or a salt bath, then double or triple tempering at 538\u2013595\u00b0C. Tempered correctly, M2 reaches about 60\u201365 HRC, with the high hardness, wear resistance, and red hardness expected from a high-speed steel. Hardness values&hellip;","rttpg_featured_image_url":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif",1254,1254,false],"landscape":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif",1254,1254,false],"portraits":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif",1254,1254,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-150x150.avif",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-300x300.avif",300,300,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-1024x1024.avif",1024,1024,true],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif",1254,1254,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad.avif",1254,1254,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/05\/M2-heat-treatment-ad-12x12.avif",12,12,true]},"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"M2 Tool Steel Heat Treatment Guide M2 tool steel is heat-treated by double preheating, austenitizing at 1190\u20131230\u00b0C, quenching in oil, air, or a salt bath, then double or triple tempering at 538\u2013595\u00b0C. Tempered correctly, M2 reaches about 60\u201365 HRC, with the high hardness, wear resistance, and red hardness expected from a high-speed steel. Hardness values&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/11688","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=11688"}],"version-history":[{"count":10,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/11688\/revisions"}],"predecessor-version":[{"id":23009,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/11688\/revisions\/23009"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media\/15110"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=11688"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}