4Cr3Mo3SiV is the designation under China’s GB/T standard, and its equivalent steels are ASTM/AISI H10 in the United States, JIS SKD7 in Japan, DIN 1.2365 in Germany, and 32CrMoV12-28. 4Cr3Mo3SiV is a medium-alloy hot work tool steel. It is designed with a good balance of strength, toughness, and wear resistance at elevated temperatures. Compared to 4Cr5MoSiV1 (H13) steel, it has higher thermal strength but slightly lower impact toughness. Its thermal stability surpasses both H13 and 3Cr2W8V (H21) steels.
1. Kémiai összetétel (GB / T 1299—2000)
| C | Si | Mn | Kr | Mo | V. | P | S |
| 0.35 – 0.45 | 0.80 – 1.20 | 0.25 – 0.70 | 3.00 – 3.75 | 2.00 – 3.00 | 0.25 – 0.75 | ≤0,030 | ≤0,030 |
2. Critical Point Temperatures of 4Cr3Mo3SiV
| Kritikus pont | Ac₁ | Ac₃ | Asszony |
| Temperature (approximate value)/°C | 820 | 900 | 310 |
3. 4Cr3Mo3SiV Steel Forging Process Specification
| Tétel | Fűtési hőmérséklet/°C | Kezdeti kovácsolási hőmérséklet/°C | Végső kovácsolási hőmérséklet/°C | Hűtési módszer |
| Acélöntvény | 1160 ~ 1180 | 1040 ~ 1170 | ≥900 | Lassú hűtés |
| Acél tuskó | 1150 ~ 1170 | 1120 ~ 1140 | ≥850 | Lassú hűtés |

Please complete the following contact form to obtain the best quotation for 4Cr3Mo3SiV/H10 steel.
4. Heat Treatment of 4Cr3Mo3SiV
4.1 Előmelegítés
| Material | Fűtési hőmérséklet/°C | Holding Time | Isothermal Time | Hűtési módszer |
| Bar Stock | 860 ~ 880 | 2h + 1min/mm | — | Furnace cool to below 500°C, then air cool |
| Kovácsolt tárgyak | 860 ~ 880 | 1h + 1min/mm | 730°C × 2h + 1min/mm | Air cool from furnace |
4.2 Kioltás
| First Preheating | Second Preheating | Austenitizing Temperature/°C | Hűtőközeg | Keménység HRC |
| 550°C uniform heating | 880°C uniform heating | 1030 ± 10 | Olaj | 55 ~ 56 |
4.3 Edzés
| First Tempering | Second Tempering | Keménység HRC |
| 610°C × 2h | 615°C × 2h | 47.0 ~ 49.0 |
5. Mechanical Properties of 4Cr3Mo3SiV
4Cr3Mo3SiV contains many carbide-forming elements such as Cr, Mo, and V. It has good toughness and exhibits high hardness, thermal strength, and wear resistance at operating temperatures of 500~600 °C. This steel has good hardenability, resistance to tempering, and thermal stability, resulting in very high toughness, high impact toughness, and fracture toughness, as well as good oxidation resistance.
5.1 Room Temperature Mechanical Properties
| Specimen Hardness HRC | Rm/MPa | ReL/MPa | A (%) | Z (%) | KU/J | K.Ic/MPa·1/2 |
| 47 ~ 49 | 1559 | 1356 | 10.1 | 34.1 | 16.9 | 41.2 |
5.2 High-Temperature Mechanical Properties
| Hőmérséklet/°C | Rm/MPa | ReL/MPa | A (%) | Z (%) | KU/J | Vickers Hardness HV |
| 300 | 1349 | 1218 | 10.4 | 29.3 | 20.5 | 471.5 |
| 600 | 888 | 779 | 20.3 | 69.8 | 25.2 | 409.0 |
| 650 | 651 | 596 | 19.5 | 60.7 | 20.9 | 360.5 |
| 700 | 298 | 261 | 31.2 | 81.6 | 23.2 | 278.5 |
5.3 Thermal Stability
| Megeresztési hőmérséklet (°C) | Holding Time (h) | Keménység (HRC) |
| 620 | 0 | 47.5 |
| 2 | 44.1 | |
| 4 | 43.8 | |
| 6 | 42.2 | |
| 8 | 41.3 | |
| 11.5 | 38.6 | |
| 14.5 | 37.6 | |
| 17.5 | 35.4 | |
| 21 | 33.8 | |
| 660 | 0 | 46.9 |
| 1 | 40.3 | |
| 2 | 34.9 | |
| 3 | 33.8 | |
| 5 | 31.5 | |
| 7 | 29.8 | |
| 9 | 29.5 | |
| 12 | 26.8 | |
| 700 | 0 | 46.6 |
| 0.5 | 33.5 | |
| 1 | 29 | |
| 1.5 | 28.3 | |
| 2 | 25.8 | |
| 3 | — |
5.4 Fatigue Performance
| Test Condition | 20°C ↔ 650°C (1000 cycles) | 20°C ↔ 700°C (1000 cycles) |
| 47 ~ 49HRC | Grade 7.6 | Grade 15.6 |
6. Applications of 4Cr3Mo3SiV
4Cr3Mo3SiV steel is widely used for various hot work tooling and components:
- Forró extrudáló szerszámok: Especially for core rods, liners, and mandrels.
- Meleg kovácsoló szerszámok: For thermal forging, precision forging, roll forging, and hammer forging dies.
- Hot Punching Dies: Used for hot punches and hot pressing dies.
- Die-Casting Molds: Suitable for aluminum, magnesium, and copper alloy die-casting molds.
- Egyéb alkalmazások: Hot cutting tools, pressure tools, and components requiring good impact resistance and hardness at elevated temperatures. It can replace 3Cr2W8V in many applications.
Get a Competitive Quote for 4Cr3Mo3SiV Tool Steel
With over 20 years of forging expertise, Aobo Steel is your trusted partner for high-performance 4Cr3Mo3SiV tool steel. We provide not just materials, but solutions. Leverage our deep industry knowledge and reliable supply chain for your project’s success.
✉ Lépjen velünk kapcsolatba az alábbi űrlap kitöltésével.