2Cr13 stainless steel is a versatile material widely used in manufacturing plastic molds, especially those that require a balance of strength, toughness, and corrosion resistance. As a low-carbon martensitic stainless steel, it is typically employed after quenching and tempering. This heat treatment enhances its mechanical properties, making it suitable for demanding applications.
One of the key advantages of 2Cr13 steel is its good machinability, which allows for efficient processing and shaping. After heat treatment, it exhibits excellent corrosion resistance, ensuring longevity even in harsh environments. And it has a good combination of strength and toughness.
1. Chemical Composition(GB/ T 094—1997)
| C | Si | Mn | Kr | S | P |
| 0.16 ~ 0.25 | ≤1.00 | ≤1.00 | 12.00 ~ 14.00 | ≤0,030 | ≤0,030 |
2. Physical Properties of 2Cr13 Stainless Steel
2.1 Kritikus hőmérsékletek
| Kritikus pont | Ac₁ | Ac₃ | Ar₁ | Asszony |
| Hőmérséklet (hozzávetőleges érték) /°C | 820 | 950 | 780 | 320 |
2.2 Elastic Modulus
| Hőmérséklet /°C | 20 | 400 | 500 | 600 |
| Elastic Modulus E/MPa | 210000 ~ 223000 | 193000 | 184000 | 172000 |
2.3 Coefficient of Linear Expansion
| Hőmérséklet /°C | 20 ~ 100 | 20 ~ 200 | 20 ~ 300 | 20 ~ 400 | 20 ~ 500 |
| Coeff. of Linear Expansion α/×10⁻⁶ ℃⁻¹ | 10.5 | 11.0 | 11.5 | 12.0 | 12.0 |
2.4 Hővezető képesség
| Hőmérséklet /°C | 20 ~ 100 | 20 ~ 200 | 20 ~ 300 | 20 ~ 400 | 20 ~ 500 |
| Hővezető képesség λ/[W/(m·K)] | 23.0 | 23.4 | 24.7 | 25.5 | 26.3 |
2.5 Electrical Resistivity of SM2Cr13 Steel
| Hőmérséklet /°C | 20 | 100 |
| Electrical Resistivity ρ/×10⁻⁶ Ω·m | 0.55 | 0.65 |
2.6 Egyéb fizikai tulajdonságok
| Sűrűség / (g/cm³) | Specific Heat Capacity cₚ / [J/(kg·K)] | Melting Point / °C |
| 7.75 | 459.8 | 1450 ~ 1510 |
3. Forging Process Specification of 2Cr13 Stainless Steel
| Fűtés | Kezdeti kovácsolási hőmérséklet/°C | Végső kovácsolási hőmérséklet/°C | Hűtés |
| Slow heating before 850°C, cold furnace charging temperature ≤800°C | 1160 ~ 1200 | ≥850 | Sand cooling or timely annealing |
Jegyzet: Due to the poor thermal conductivity of the steel, it should be heated slowly when the temperature is below 856°C.
4. Cold working
It has good deep drawing and stamping processability in a cold state. After processing, stress relief annealing should be performed. The process is to heat the workpiece to 730 ~ 780°C and then air cool it.

Please fill out the following form to contact us for the most competitive quotation on 2Cr13 stainless steel.
5. Heat treatment of 2Cr13 Stainless Steel
5.1 Preheating
| Pre-heat Treatment Process | Heating Temperature (°C) | Hűtési módszer | Hardness (HBW) |
| Lágyító hőkezelés | 750 ~ 800 | Furnace Cooling | — |
| Teljes lágyítás | 860 ~ 900 | Furnace Cooling | 160 ~ 187 |
5.2 Quenching and Tempering Process Specification
| Quenching Specification | Tempering Specification | ||||
| Kioltási hőmérséklet (°C) | Hűtési módszer | Keménység (HRC) | Megeresztési hőmérséklet (°C) | Hűtési módszer | Keménység (HRC) |
| 1000 ~ 1050 | Oil or Water Cooling | ≥45 | 660 ~ 670 | Léghűtés | 20 ~ 23 |
Relationship Between Tempering Temperature and Hardness
| Megeresztési hőmérséklet (°C) | Kioltás után | 200 | 300 | 400 | 500 | 550 | 600 | 650 |
| Keménység (HRC) | 47 | 46 | 45 | 44 | 43 | 37 | 30 | 24 |
Note: 1050°C oil quenching.
6. Mechanical Properties of 2Cr13 Stainless Steel
2Cr13 is a martensitic stainless steel with high toughness and deformation resistance, and good machinability. After heat treatment, it has high strength, hardness, and excellent wear resistance.
1) Mechanical properties at different tempering temperatures.
| Tempering Temperature /°C | Rm /MPa | ReL /MPa | Z (%) | A (%) |
| 300 | 1580 | 1430 | 10 | 5 |
| 400 | 1550 | 1390 | 11 | 5.5 |
| 500 | 1460 | 1250 | 15 | 7.5 |
| 600 | 1150 | 900 | 22 | 14 |
| 700 | 780 | 580 | 27 | 19 |
| 800 | 800 | 600 | 26 | 16 |
Note: 100°C oil quenching.
2) High-temperature mechanical properties
| Hőkezelés | Test Temperature (°C) | Rm (MPa) | ReL (MPa) | A (%) | Z (%) | egyK. (J/cm²) |
| Quenching at 1000 ~ 1020°C, Tempering at 720 ~ 750°C | 20 | 720 | 520 | 21 | 68 | 65 ~ 175 |
| 300 | 555 | 400 | 18 | 66 | 120 | |
| 400 | 530 | 405 | 16.5 | 58.5 | 205 | |
| 450 | 495 | 380 | 17.5 | 57 | 240 | |
| 470 | 495 | 420 | 22.5 | 71 | ||
| 500 | 440 | 365 | 32.5 | 75 | 250 | |
| 550 | 350 | 285 | 36.5 | 83.5 | 223 |
3) Room temperature mechanical properties
| Section Size / mm | Hőkezelés | R<sub>m</sub> / MPa | R<sub>eL</sub> / MPa | A (%) | Z (%) | a<sub>k</sub> / (J/cm²) | Keménység HBW |
| ≤60 | 1000 ~ 1050℃ Quenching (Oil, Water cooling), 600 ~ 770℃ Tempering, Oil, Water, Air cooling | ≥660 | ≥450 | ≥16 | ≥55 | ≤80 | ≤197 |
| 1000 ~ 1050℃, Quenching (Oil, Water cooling), 660 ~ 770℃ Tempering | 660 ~ 1155 | 450 ~ 975 | 16 ~ 33.6 | 55 ~ 78 | 80 ~ 267 | 126 ~ 197¹ | |
| 860℃ Annealing | 500 | 250 | 22 | 45 | 90 | ||
| 1050℃ Air Quenching, 500℃ Tempering | 1250 | 950 | 7 | 55 | 50 | ||
| 1050℃ Air Quenching, 600℃ Tempering | 850 | 650 | 10 | 63.5 | 70 | ||
| 1050℃ Oil Quenching, 660℃ Tempering | 860 | 710 | 19 | 66.5 | 130 | ||
| 1050℃ Oil Quenching, 770℃ Tempering | 820 | 700 | 18 | 150 |
4) Creep Rupture Strength
| Test Temperature /°C | 450 | 470 | 500 | 530 |
| R_m (1000h) /MPa | 330 | 260 | 230 | 160 |
| R_m (10000h) /MPa | 296 | 215 | 195 | 105 |
| R_m (100000h) /MPa | 260 | 190 | 160 | 76 |
5) creep strength
| Test Temperature /°C | 450 | 475 | 500 | 550 |
| σ-1 (100000h) /MPa | 128 | 75 | 48 | 38 |
Jegyzet: The test steel was air-cooled at 1000 ~ 1020°C and tempered at 720~730 °C.
5) Corrosion Resistance
| Közepes | Concentration (mass fraction, %) | Hőmérséklet/°C | Test Duration/h | Corrosion Depth/(mm/a) |
| Salétromsav | 5 | 20 | — | <0.1 |
| Salétromsav | 5 | Forró | — | 3.00~10.0 |
| Salétromsav | 20 | 20 | — | <0.1 |
| Salétromsav | 20 | Forró | — | 1.0~3.0 |
| Salétromsav | 30 | Forró | — | <3.0 |
| Salétromsav | 50 | 20 | — | <0.1 |
| Salétromsav | 50 | Forró | — | <3.0 |
| Salétromsav | 65 | 20 | — | <0.1 |
| Salétromsav | 65 | Forró | — | 3~10 |
| Salétromsav | 90 | 20 | — | <0.1 |
| Salétromsav | 90 | Forró | — | <10.0 |
| Citric acid | 5 | 140 | — | <10.0 |
| Citric acid | 10 | Forró | — | >10.0 |
| Lactic acid | Relative density 1.01 ~ 1.04 | Forró | 72 | >10.0 |
| Lactic acid | Relative density 1.04 | 20 | 600 | 0.27 |
| Formic acid | 10 ~ 50 | 20 | — | <0.1 |
| Formic acid | 10 ~ 50 | Forró | — | >10.0 |
| Salicylic acid | 20 | — | <0.1 | |
| Stearic acid | >100 | — | <0.1 | |
| Pyrogallic acid | Dilute ~ concentrated solution | 20 | — | <0.1 |
| Carbon dioxide and carbonic acid | Dry | <100 | — | <0.1 |
| Carbon dioxide and carbonic acid | Humid | <100 | — | <0.1 |
| Cellulose | During steaming | — | 190 | 2.59 |
| Cellulose | In the slurry tank | — | 240 | 0.369 |
| Cellulose | Together with peracetic acid in the tank | — | 240 | 22.85 |
| Sodium hydroxide | 20 | 50 | — | <0.1 |
| Sodium hydroxide | 20 | Forró | — | <1.0 |
| Sodium hydroxide | 30 | 100 | — | <1.0 |
| Sodium hydroxide | 40 | 100 | — | <1.0 |
| Sodium hydroxide | 50 | 100 | — | 1.0~3.0 |
| Sodium hydroxide | 60 | 90 | — | <1.0 |
| Sodium hydroxide | 90 | 300 | — | >10.0 |
| Sodium hydroxide | Molten | 318 | — | >10.0 |
| Boric acid | 50 ~ Saturated solution | 100 | — | <0.1 |
| Ecetsav | 1 | 90 | — | <0.1 |
| Ecetsav | 5 | 20 | — | <1.0 |
| Ecetsav | 5 | Forró | — | >10.0 |
| Ecetsav | 10 | 20 | — | <1.0 |
| Ecetsav | 10 | Forró | — | >10.0 |
| Tartaric acid | 10 ~ 50 | 20 | — | <0.1 |
| Tartaric acid | 10 ~ 50 | Forró | — | <1.0 |
| Tartaric acid | Saturated solution | Forró | — | <10.0 |
| Citric acid | 1 | 20 | — | >0.1 |
| Citric acid | 1 | Forró | — | — |
| Potassium hydroxide | 25 | Forró | — | — |
| Potassium hydroxide | 50 | 20 | — | — |
| Potassium hydroxide | 50 | Forró | — | — |
| Potassium hydroxide | 68 | 120 | — | — |
| Potassium hydroxide | Molten | 300 | — | >10.0 |
| Ammonia | Solution and gas | 20 ~ 100 | — | <0.1 |
| Ammonium nitrate | approx 65 | 20 | — | 0.0011 |
| Ammonium nitrate | approx 65 | 125 | — | 1.43 |
| Ammonium chloride | Saturated solution | Forró | 1269 | <10.0 |
| Hydrogen peroxide | 20 | 20 | 110 | 0 |
| Iodine | Dry | 20 | — | <0.1 |
| Iodine | Solution | 20 | — | >10.0 |
| Bromoform | Vapor | 60 | — | <0.1 |
| Potassium nitrate | 25 ~ 50 | 20 | — | <0.1 |
| Potassium nitrate | 25 ~ 50 | Forró | — | <10.0 |
| Potassium nitrate | 10 | 20 | — | 0.07 |
| Potassium sulfate | 10 | Forró | — | 1.18 |
| Silver nitrate | 10 | Forró | 720 | <0.1 |
| Silver nitrate | Molten | 250 | 96 | >10.0 |
| Sodium peroxide | 10 | 20 | — | <10.0 |
| Sodium peroxide | 10 | Forró | — | >10.0 |
| Alum | 10 | 20 | — | 0.1 ~ 1.0 |
| Alum | 10 | 100 | — | <10.0 |
| Potassium dichromate | 25 | 20 | — | <0.1 |
| Potassium dichromate | 25 | Forró | — | >10.0 |
| Potassium chlorate | Saturated solution | 100 | — | <0.1 |
6. Equivalent Grades
- German DIN: Material number 1.4021, grade X20Cr13
- British BS: Grade S62
- British EN: Grades 56B/56C
- French AFNOR: Grade Z20C13
- American AISI: 420
GYIK
2Cr13 is a martensitic stainless steel. Its typical chemical composition includes 0.16-0.25% Carbon (C), ≤0.60% Silicon (Si), ≤0.80% Manganese (Mn), 12.00-14.00% Chromium (Cr), ≤0.030% Sulfur (S), and ≤0.035% Phosphorus (P). It is often used for parts requiring high stress, such as turbine blades, hot oil pump shafts and impellers, and hydraulic press valves.
2Cr13 is good for applications requiring excellent corrosion resistance, polishability, high strength, and wear resistance after heat treatment. It’s suitable for parts under high stress and in certain corrosive environments, including paper industry components, medical instruments, and household items like cutlery. However, its weldability can be poor, and it may have lower toughness and corrosion resistance compared to some other stainless steels like 12Cr13.
In practical terms, 2Cr13 stainless steel is often directly comparable to or the same as AISI/SAE 420 stainless steel. Both have a similar chromium content of 12-14% and carbon content typically ranging from 0.15% to 0.25%. Both are martensitic grades and are hardenable.
The primary difference between 2Cr13 and 3Cr13 stainless steel lies in their carbon content.
2Cr13: Contains 0.16-0.25% Carbon.
3Cr13: Contains a higher carbon content of 0.26-0.35%. This higher carbon content in 3Cr13 results in greater strength, hardness, and hardenability compared to 2Cr13 (and 12Cr13) after quenching. However, 3Cr13’s toughness and corrosion resistance may be slightly lower than 2Cr13. Both are martensitic stainless steels.
Get a Competitive Quote for 2Cr13 Stainless Steel
With over 20 years of forging expertise, Aobo Steel is your trusted partner for high-performance 2Cr13 stainless steel. We provide not just materials, but solutions. Leverage our deep industry knowledge and reliable supply chain for your project’s success.
✉ Lépjen velünk kapcsolatba az alábbi űrlap kitöltésével.
Fedezze fel további termékeinket
D2/1.2379/SKD11
D3/1.2080/SKD1
D6/1.2436/SKD2
A2/1.23663/SKD12
O1/1.2510/SKS3
O2/1,2842
S1/1.2550
S7/1.2355
DC53
H13/1.2344/SKD61
H11/1.2343/SKD6
H21/1.2581/SKD7
L6/1.2714/SKT4
M2/1.3343/SKH51
M35/1.3243/SKH55
M42/1.3247/SKH59
P20/1.2311
P20+Ni/1,2738
420/1.2083/2Cr13
422 rozsdamentes acél
52100 csapágyacél
440C rozsdamentes acél
4140/42CrMo4/SCM440
4340/34CrNiMo6/1.6582
4130
5140/42Cr4/SCR440
SCM415