{"id":21355,"date":"2026-10-08T18:49:47","date_gmt":"2026-10-08T10:49:47","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21355"},"modified":"2026-10-19T22:51:26","modified_gmt":"2026-10-19T14:51:26","slug":"galling-of-stainless-tool-steels","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/es\/galling-of-stainless-tool-steels\/","title":{"rendered":"Gripado de aceros inoxidables y cu\u00e1nto esfuerzo requiere"},"content":{"rendered":"<h1 id=\"h-galling-of-stainless-steels-and-how-much-stress-it-takes\" class=\"wp-block-heading\">Gripado de aceros inoxidables y cu\u00e1nto esfuerzo requiere<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">El gripado es la soldadura en fr\u00edo de puntos microsc\u00f3picos altos entre dos superficies deslizantes, y es la raz\u00f3n por la que una pieza de acero inoxidable que se mov\u00eda libremente en el taller se agarrota en la m\u00e1quina. Las cinco familias de acero inoxidable son susceptibles, incluidos los grados martens\u00edticos que un taller de herramientas compra como 420 y 440C. Tambi\u00e9n se mide. El ensayo de bot\u00f3n sobre bloque devuelve un esfuerzo umbral de gripado para cada grado y condici\u00f3n, y la tabla publicada cubre cuatro familias y diecis\u00e9is designaciones de aleaci\u00f3n, suficiente para responder qu\u00e9 inoxidable combinar con qu\u00e9.<\/p>\n\n\n\n<h2 id=\"h-the-threshold-galling-stress-grade-by-grade\" class=\"wp-block-heading\">El esfuerzo umbral de gripado, grado por grado<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">En el ensayo de bot\u00f3n sobre bloque, un bot\u00f3n cargado se rota contra un bloque del mismo material hasta que la superficie se desgarra; la tensi\u00f3n de contacto en ese punto es el esfuerzo umbral de gripado. Un n\u00famero m\u00e1s alto es mejor. Las entradas marcadas como no gripantes recorrieron todo el rango del ensayo sin desgarro, por lo que comparten un valor, y las dos columnas de unidades reproducen la impresi\u00f3n de origen. La dureza se da como la da la fuente, en Rockwell B o Rockwell C.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Grado<\/th><th class=\"has-text-align-left\" data-align=\"left\">Condici\u00f3n<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza<\/th><th class=\"has-text-align-left\" data-align=\"left\">MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">ksi<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\">Austen\u00edtico<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S20161<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">104 (a)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (a)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S21800<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">104 (a)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (a)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S28200<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">166<\/td><td class=\"has-text-align-left\" data-align=\"left\">24<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S28200<\/td><td class=\"has-text-align-left\" data-align=\"left\">Estirado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">35 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S20910<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">97 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S20900<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S24100<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">23 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">97<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S30430<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">74 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">86 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">Estirado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">17<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">82 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">Estirado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 303<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">85 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">138<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">104<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">N08020<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">87 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\">Martens\u00edtico<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S42010<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 204 \u00b0C (400 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">50 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">104 (a)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (a)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S42010<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 260 \u00b0C (500 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">47 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 410<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">87 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 410<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 260 \u00b0C (500 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">43 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">21<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 416<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">21<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 416<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 316 \u00b0C (600 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">37 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 416<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 538 \u00b0C (1000 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">32 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">42<\/td><td class=\"has-text-align-left\" data-align=\"left\">6<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 420<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 204 \u00b0C (400 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">51 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">18<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 420<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 260 \u00b0C (500 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">49 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 440C<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 260 \u00b0C (500 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">55 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">18<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\">Endurecible por precipitaci\u00f3n<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45500<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 510 \u00b0C (950 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">48 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45500<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 566 \u00b0C (1050 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">43 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">59<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45500<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 621 \u00b0C (1150 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">36 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">28<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">29 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">69<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 480 \u00b0C (895 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">43 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 566 \u00b0C (1050 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">17<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 621 \u00b0C (1150 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">33 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S17400<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 480 \u00b0C (895 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">45 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">69<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S17400<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 621 \u00b0C (1150 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">34 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S13800<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 538 \u00b0C (1000 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">46 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">21<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S66286<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envejecido a 718 \u00b0C (1325 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\">Ferr\u00edtico y d\u00faplex<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S18200<\/td><td class=\"has-text-align-left\" data-align=\"left\">Estirado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">98 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 430F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 430<\/td><td class=\"has-text-align-left\" data-align=\"left\">Estirado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">98 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 329<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">25 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Esfuerzo umbral de gripado de aceros inoxidables autoapareados en el ensayo de bot\u00f3n sobre bloque, ASTM G98, acabado rectificado sin lubricar, reproducido del ASM Handbook, Volumen 18. Las entradas marcadas con (a) no presentaron gripado dentro del rango del ensayo. Los valores se imprimen tal como figuran en la fuente.<\/em><\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Gripado de los aceros inoxidables, PDF imprimible<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">El esfuerzo umbral de gripado para cada familia de inoxidable, la clasificaci\u00f3n de materiales para desgaste adhesivo, el volumen perdido por las aleaciones comunes y el efecto de la temperatura, en un PDF con nuestros datos de contacto.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Galling-Of-Stainless-Steels.pdf\">Descargar PDF<\/a><\/div>\n<\/div>\n<\/div>\n\n\n\n<h2 id=\"h-what-the-ranking-says\" class=\"wp-block-heading\">Lo que dice la clasificaci\u00f3n<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Entre los grados austen\u00edticos, las aleaciones cromo-manganeso-nitr\u00f3geno superan a las aleaciones cromo-n\u00edquel de dureza similar. S28200, S20161 y S21800 muestran los umbrales m\u00e1s altos de la familia, mientras que N08020, la aleaci\u00f3n rica en n\u00edquel, muestra el m\u00e1s bajo con 14 MPa. La fuente lo atribuye a dos efectos de aleaci\u00f3n. El n\u00edquel perjudica la resistencia al gripado, mientras que el silicio ayuda, lo que explica ambos extremos de la tabla. El tipo 303, el grado de f\u00e1cil mecanizado, se sit\u00faa alto con 138 MPa debido a su qu\u00edmica y superficie mecanizada, y recuerda que un grado elegido por una propiedad trae otras propiedades consigo.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Endurecer un grado austen\u00edtico mediante estirado en fr\u00edo empeora su resistencia al gripado, no la mejora. El Tipo 304 cae de 55 MPa recocido a 86 HRB a 17 MPa estirado en fr\u00edo a 27 HRC, y S28200 cae de 166 MPa a 62 MPa con el mismo cambio. Esta es la l\u00ednea m\u00e1s contraintuitiva de la tabla, y se deriva del mecanismo. La resistencia al gripado en estas aleaciones proviene de la capacidad de endurecerse por deformaci\u00f3n justo en el contacto, y un grado que ya ha sido trabajado en fr\u00edo ha gastado esa capacidad antes de que la pieza entrara en servicio.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Entre los grados martens\u00edticos, una mayor dureza de trabajo no produce por s\u00ed sola un umbral m\u00e1s alto, y las dos condiciones del Tipo 420 lo muestran claramente. Revenido a 204 C hasta 51 HRC, devuelve 25 MPa; revenido a 260 C hasta 49 HRC, devuelve 55 MPa, por lo que la condici\u00f3n m\u00e1s blanda es mejor. El Tipo 440C a 55 HRC es la entrada martens\u00edtica m\u00e1s fuerte con 125 MPa, lo que coincide con su reputaci\u00f3n como acero inoxidable para herramientas de contacto deslizante. S42010 no present\u00f3 gripado a 50 HRC, y la cifra de dureza por s\u00ed sola no lo habr\u00eda predicho.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Los grados de endurecimiento por precipitaci\u00f3n siguen su temperatura de envejecimiento m\u00e1s que su contenido de aleaci\u00f3n. S45500 pierde umbral de forma constante a medida que aumenta la temperatura de envejecimiento, de 90 MPa a 510 C a 59 MPa a 566 C y 28 MPa a 621 C, y S45000 hace lo mismo de 69 MPa a 14 MPa. Una pieza reenvejecida a mayor temperatura para ganar ductilidad cede resistencia al gripado al hacerlo.<\/p>\n\n\n\n<h2 id=\"h-one-design-assumption-that-does-not-survive-the-data\" class=\"wp-block-heading\">Una suposici\u00f3n de dise\u00f1o que no sobrevive a los datos<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Una regla general com\u00fan es que una gran diferencia de dureza entre dos piezas acopladas previene el gripado. Los datos de desgaste publicados no lo respaldan. Probados contra seis aleaciones de contracara diferentes, el tipo 440C a 57 HRC y S21800 a 95 HRB fueron buenas selecciones independientemente de la dureza del material contra el que corrieron. La elecci\u00f3n de la mejor aleaci\u00f3n, no el tama\u00f1o de la brecha de dureza, determina el resultado. Dentro de un mismo grado, la dureza sigue importando, y el mismo ensayo muestra al tipo 440C perdiendo 0,7 mm3 a 56 HRC y 44,1 mm3 a 26,5 HRC, por lo que una vez elegido el grado, el tratamiento de endurecimiento no es opcional.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Los grados austen\u00edticos que endurecen por deformaci\u00f3n m\u00e1s r\u00e1pido tambi\u00e9n resisten mejor el desgaste adhesivo, por lo que S20161 y S21800 se sit\u00faan en la cima de la clasificaci\u00f3n de desgaste adhesivo en el ensayo de cilindros cruzados y por lo que el tipo martens\u00edtico 410 a 24,5 HRC se sit\u00faa en el fondo. La misma clasificaci\u00f3n coloca un acero para herramientas com\u00fan al frente del grupo.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Material<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza<\/th><th class=\"has-text-align-left\" data-align=\"left\">A 105 rev\/min<\/th><th class=\"has-text-align-left\" data-align=\"left\">A 415 rev\/min<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">acero para herramientas D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">61 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.46<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.34<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AISI 4337<\/td><td class=\"has-text-align-left\" data-align=\"left\">52 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.73<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.48<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Stellite 6B<\/td><td class=\"has-text-align-left\" data-align=\"left\">48 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.27<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Acero al Mn Hadfield<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.41<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Bronce al Al (10,5%)<\/td><td class=\"has-text-align-left\" data-align=\"left\">87 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.52<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Aluminio Tipo 6061-T6<\/td><td class=\"has-text-align-left\" data-align=\"left\">59 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.15<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AISI 4130<\/td><td class=\"has-text-align-left\" data-align=\"left\">47 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.44<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.80<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Astralloy V<\/td><td class=\"has-text-align-left\" data-align=\"left\">46 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">213.58<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.22<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 440C<\/td><td class=\"has-text-align-left\" data-align=\"left\">57 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.81<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.54<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S21800<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.79<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.58<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">90 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.95<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.68<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Clasificaci\u00f3n relativa de la resistencia al desgaste adhesivo de materiales trabajados, reproducida del ASM Handbook, Volumen 18. La p\u00e9rdida de peso se expresa en miligramos por mil ciclos en el ensayo de cilindros cruzados, ASTM G83, a 71 N. A 61 HRC, la mejor entrada de la tabla es el <a href=\"https:\/\/aobosteel.com\/es\/d2-steel-properties\/\">acero para herramientas D2<\/a>, por delante de la aleaci\u00f3n de recubrimiento duro base cobalto en la tercera fila.<\/em><\/p>\n\n\n\n<h2 id=\"h-temperature-moves-the-answer\" class=\"wp-block-heading\">La temperatura cambia la respuesta<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">El desgaste adhesivo no es una propiedad fija de un par, porque tanto la pel\u00edcula de \u00f3xido como la tensi\u00f3n de fluencia cambian con la temperatura. S21800 mejora a medida que la junta funciona m\u00e1s caliente, con la p\u00e9rdida de volumen cayendo de 2,6 mm3 a 80 C a 2,2 mm3 a 315 C y 1,3 mm3 a 540 C, mientras que el tipo 304 se mantiene similar en el mismo rango. El tipo 410 se comporta de manera opuesta. A 95 HRB, pierde 282,8 mm3 a 80 C, y endurecerlo a 40 HRC lo reduce a 42,1 mm3, como con un grado martens\u00edtico, incluso cuando el umbral de gripado sugiere que el revenido m\u00e1s blando es mejor. La aleaci\u00f3n de recubrimiento duro base cobalto en la misma serie comienza baja y aumenta con la temperatura, por lo que no es la respuesta autom\u00e1tica a cualquier temperatura.<\/p>\n\n\n\n<h2 id=\"h-what-to-do-about-a-stainless-tool-that-seizes\" class=\"wp-block-heading\">Qu\u00e9 hacer con una herramienta inoxidable que se agarrota<\/h2>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Medida<\/th><th class=\"has-text-align-left\" data-align=\"left\">Por qu\u00e9 funciona<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Elija el grado de la lista medida<\/td><td class=\"has-text-align-left\" data-align=\"left\">La elecci\u00f3n del grado mueve el umbral de tensi\u00f3n de gripado por un factor de veinte o m\u00e1s, por lo que es la primera decisi\u00f3n y no la \u00faltima.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Haga que el par sea dis\u00edmil<\/td><td class=\"has-text-align-left\" data-align=\"left\">Una pieza de acero inoxidable que trabaja contra una familia de materiales diferente elimina por completo el peor caso de gripado entre materiales iguales.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">No conf\u00ede en el trabajo en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">El estirado en fr\u00edo de un grado austen\u00edtico eleva su dureza y reduce su resistencia al gripado al mismo tiempo, que es lo contrario de lo que sugiere el valor de dureza.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Mantenga la superficie rectificada y libre de residuos<\/td><td class=\"has-text-align-left\" data-align=\"left\">Los valores umbral publicados se miden sobre un acabado rectificado sin lubricaci\u00f3n, por lo que una superficie desgarrada o limada a mano queda por debajo de ellos.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Lubrique donde la aplicaci\u00f3n lo permita<\/td><td class=\"has-text-align-left\" data-align=\"left\">Una pel\u00edcula de cualquier tipo separa las asperezas que de otro modo se soldar\u00edan en fr\u00edo, y el desgaste adhesivo es el mecanismo que esa pel\u00edcula interrumpe.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Vigile la temperatura de servicio<\/td><td class=\"has-text-align-left\" data-align=\"left\">Los grados austen\u00edticos mantienen o mejoran su resistencia al desgaste adhesivo a medida que la junta funciona m\u00e1s caliente, mientras que las aleaciones endurecibles la pierden.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Medidas contra el gripado en utillaje de acero inoxidable y piezas acopladas, de ASM Handbook, Volumen 18. Los m\u00e9todos de ensayo publicados detr\u00e1s de la tabla son el ensayo de cribado de bot\u00f3n sobre bloque y, para conexiones roscadas, un ensayo de montaje y desmontaje sobre la conexi\u00f3n real.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Cuando la pieza es acero para herramientas en lugar de inoxidable, el mismo mecanismo determina el grado, y la respuesta se expone en <a href=\"https:\/\/aobosteel.com\/es\/adhesive-wear-resistant-tool-steels\/\">aceros para herramientas resistentes al desgaste adhesivo<\/a>. Los dos aceros para herramientas inoxidables que llevan estos datos en un taller de utillaje son el <a href=\"https:\/\/aobosteel.com\/es\/440c-stainless-steel\/\">acero inoxidable 440C<\/a>, el umbral m\u00e1s alto de la familia martens\u00edtica, y el <a href=\"https:\/\/aobosteel.com\/es\/420-stainless-steel\/\">acero inoxidable 420<\/a>, que necesita el revenido correcto para dar su mejor resultado.<\/p>\n\n\n\n<h2 id=\"h-grades-and-stock\" class=\"wp-block-heading\">Grados y existencias<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">El acero inoxidable para herramientas se compra por dos propiedades a la vez, y el desgaste o el gripado es solo la primera. La <a href=\"https:\/\/aobosteel.com\/es\/stainless-steel-corrosion-resistance-chart\/\">tabla de resistencia a la corrosi\u00f3n de aceros inoxidables<\/a>\u00a0cubre la corrosi\u00f3n, la <a href=\"https:\/\/aobosteel.com\/es\/stainless-steel-composition-chart\/\">tabla de composici\u00f3n del acero inoxidable<\/a> cubre la composici\u00f3n, y la <a href=\"https:\/\/aobosteel.com\/es\/stainless-steel-sensitization\/\">sensibilizaci\u00f3n del acero inoxidable<\/a> cubre lo que el calor hace al cromo en servicio.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Si el da\u00f1o es una mancha o picadura en lugar de una superficie desgarrada, el mecanismo difiere, y el diagn\u00f3stico est\u00e1 en la <a href=\"https:\/\/aobosteel.com\/es\/tool-steel-pitting-corrosion\/\">corrosi\u00f3n por picadura en acero para herramientas<\/a>, con el caso de rendija en la <a href=\"https:\/\/aobosteel.com\/es\/mold-steel-crevice-corrosion\/\">corrosi\u00f3n por rendija del acero para moldes<\/a>. Cuando la superficie se desgarr\u00f3 porque dos piezas se mov\u00edan con fretting en lugar de deslizarse, el patr\u00f3n se describe en el <a href=\"https:\/\/aobosteel.com\/es\/fretting-wear-tool-steel\/\">desgaste por fretting en utillaje<\/a>, y cuando un troquel fall\u00f3 por una raz\u00f3n distinta a que la pieza se le pegara, la lista de mecanismos est\u00e1 en el <a href=\"https:\/\/aobosteel.com\/es\/die-wear-and-failure-mechanisms\/\">desgaste y mecanismos de falla de matrices<\/a>.<\/p>\n\n\n\n<h3 id=\"h-before-you-use-these-values\" class=\"wp-block-heading\">Antes de usar estos valores<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Esta p\u00e1gina es un resumen de referencia de la pr\u00e1ctica publicada y no es una especificaci\u00f3n de Aobo Steel. Los umbrales y las cifras de desgaste se reproducen de las tablas de origen y se midieron sobre probetas de laboratorio preparadas, por lo que el acabado superficial, el ajuste, la lubricaci\u00f3n y la geometr\u00eda de contacto real los modificar\u00e1n. La selecci\u00f3n de grado para un trabajo de utillaje inoxidable se confirma en el trabajo.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fuente: ASM Handbook, Volume 18, Friction, Lubrication, and Wear Technology, ASM International, 1992.<\/p>","protected":false},"excerpt":{"rendered":"<p>Galling of Stainless Steels and How Much Stress It Takes Galling is the cold welding of microscopic high points between two sliding surfaces, and it&#8217;s why a stainless part that ran freely in the workshop seizes on the machine. All five families of stainless steel are susceptible, including the martensitic grades a tool shop buys [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21355","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Galling of Stainless Steels: Threshold Stress Data<\/title>\n<meta name=\"description\" content=\"The threshold galling stress of every stainless family, the ranking for adhesive wear, and the two galling assumptions the measured data do not support.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/es\/galling-of-stainless-tool-steels\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Galling of Stainless Steels and How Much Stress It Takes\" \/>\n<meta property=\"og:description\" content=\"The threshold galling stress of every stainless family, the ranking for adhesive wear, and the two galling assumptions the measured data do not support.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/es\/galling-of-stainless-tool-steels\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-19T14:51:26+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"9 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Galling of Stainless Steels and How Much Stress It Takes\",\"datePublished\":\"2026-10-08T10:49:47+00:00\",\"dateModified\":\"2026-10-19T14:51:26+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\"},\"wordCount\":1669,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"es\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\",\"name\":\"Galling of Stainless Steels: Threshold Stress Data\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-08T10:49:47+00:00\",\"dateModified\":\"2026-10-19T14:51:26+00:00\",\"description\":\"The threshold galling stress of every stainless family, the ranking for adhesive wear, and the two galling assumptions the measured data do not support.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Galling of Stainless Steels and How Much Stress It Takes\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/es\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Gripado de aceros inoxidables: datos de tensi\u00f3n umbral","description":"El umbral de tensi\u00f3n de gripado de cada familia de acero inoxidable, la clasificaci\u00f3n frente al desgaste adhesivo y las dos hip\u00f3tesis de gripado que los datos medidos no respaldan.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/es\/galling-of-stainless-tool-steels\/","og_locale":"es_ES","og_type":"article","og_title":"Galling of Stainless Steels and How Much Stress It Takes","og_description":"The threshold galling stress of every stainless family, the ranking for adhesive wear, and the two galling assumptions the measured data do not support.","og_url":"https:\/\/aobosteel.com\/es\/galling-of-stainless-tool-steels\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-19T14:51:26+00:00","twitter_card":"summary_large_image","twitter_misc":{"Tiempo de lectura":"9 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Galling of Stainless Steels and How Much Stress It Takes","datePublished":"2026-10-08T10:49:47+00:00","dateModified":"2026-10-19T14:51:26+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/"},"wordCount":1669,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"es"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/","url":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/","name":"Gripado de aceros inoxidables: datos de tensi\u00f3n umbral","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-08T10:49:47+00:00","dateModified":"2026-10-19T14:51:26+00:00","description":"El umbral de tensi\u00f3n de gripado de cada familia de acero inoxidable, la clasificaci\u00f3n frente al desgaste adhesivo y las dos hip\u00f3tesis de gripado que los datos medidos no respaldan.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Galling of Stainless Steels and How Much Stress It Takes"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Galling of Stainless Steels and How Much Stress It Takes Galling is the cold welding of microscopic high points between two sliding surfaces, and it&#8217;s why a stainless part that ran freely in the workshop seizes on the machine. All five families of stainless steel are susceptible, including the martensitic grades a tool shop buys&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Galling of Stainless Steels and How Much Stress It Takes Galling is the cold welding of microscopic high points between two sliding surfaces, and it&#8217;s why a stainless part that ran freely in the workshop seizes on the machine. All five families of stainless steel are susceptible, including the martensitic grades a tool shop buys&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/21355","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/comments?post=21355"}],"version-history":[{"count":6,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/21355\/revisions"}],"predecessor-version":[{"id":23703,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/21355\/revisions\/23703"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/media?parent=21355"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}