{"id":20886,"date":"2026-10-04T07:59:09","date_gmt":"2026-10-03T23:59:09","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20886"},"modified":"2026-10-07T07:08:25","modified_gmt":"2026-10-06T23:08:25","slug":"cold-work-tool-steel-heat-treatment","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/es\/cold-work-tool-steel-heat-treatment\/","title":{"rendered":"Tratamiento t\u00e9rmico del acero para herramientas de trabajo en fr\u00edo"},"content":{"rendered":"\n<style> :root{ --aobo-accent:#2563eb; --aobo-accent-dark:#1e1e2e; --aobo-blue:#0c56d0; --aobo-blue-dark:#073b91; --aobo-text:#333; --aobo-muted:#888; --aobo-border:#e5e7eb; --aobo-border-dark:#ddd; --aobo-stripe:#f7f7f9; --aobo-hover:#e8f0fe; --aobo-radius:8px; --aobo-radius-sm:6px; --aobo-orange:#f59e0b; --aobo-fill:#e9ecef; } *{box-sizing:border-box;} html{-webkit-text-size-adjust:100%;} body{margin:0;background:#fff;color:var(--aobo-text); font-family:-apple-system,BlinkMacSystemFont,\"Segoe UI\",Roboto,\"Helvetica Neue\",Arial,sans-serif; font-size:15px;line-height:1.6;} \/* Root scope \u2014 WordPress theme guard *\/ .ts-props{color:var(--aobo-text);background:transparent;padding:0;box-sizing:border-box;line-height:1.6;} .ts-props *{box-sizing:border-box;} .ts-props button,.ts-props input[type=\"text\"]{ background:none !important;border:none !important;border-radius:0 !important;padding:0 !important; margin:0 !important;font-size:inherit !important;font-weight:inherit !important; letter-spacing:normal !important;text-transform:none !important;box-shadow:none !important; line-height:inherit !important;text-decoration:none !important;} .aobo-wrap{max-width:1160px;margin:0 auto;} \/* Hero *\/ .ts-hero{background:#fff;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);overflow:hidden;} .ts-hero-top{padding:1.5em;background:var(--aobo-stripe);border-bottom:1px solid var(--aobo-border);} .ts-kicker{display:inline-flex;align-items:center;gap:6px;color:var(--aobo-accent);background:var(--aobo-hover); border:1px solid var(--aobo-border);border-radius:var(--aobo-radius-sm);padding:4px 8px; font-size:.85em;font-weight:600;margin-bottom:.8em;} .ts-kicker span{width:6px;height:6px;background:var(--aobo-orange);border-radius:50%;display:inline-block;} .ts-hero h1{margin:0;font-size:2rem;line-height:1.3;color:var(--aobo-text);text-align:center;} .ts-hero-top p{margin:.6em auto 0;max-width:820px;font-size:.9em;line-height:1.6;color:var(--aobo-muted);text-align:center;} \/* Tool area *\/ .ts-tool-area{padding:1.5em;} \/* Legend *\/ .ts-legend{display:flex;flex-wrap:wrap;gap:8px;margin-bottom:1em;} .ts-legend > span{display:inline-flex;align-items:center;gap:5px;font-size:.8em;color:var(--aobo-muted); background:var(--aobo-stripe);border:1px solid var(--aobo-border);border-radius:var(--aobo-radius-sm); padding:3px 8px;} .ts-legend b{color:var(--aobo-text);font-weight:600;} .ts-legend .ts-dot{width:9px;height:9px;border-radius:50%;background:var(--aobo-accent);display:inline-block; padding:0;border:0;gap:0;} \/* Controls *\/ .ts-controls{display:flex;flex-wrap:wrap;gap:10px;align-items:center;background:var(--aobo-stripe); border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);padding:1em;margin-bottom:1.2em;} .ts-search{flex:1 1 220px;max-width:340px;position:relative;} .ts-props .ts-search input{width:100% !important;border:1px solid var(--aobo-border-dark) !important; border-radius:var(--aobo-radius-sm) !important;padding:.5em .6em .5em 2em !important; font-size:.92em !important;color:var(--aobo-text) !important;background:#fff !important; outline:none !important;box-shadow:none !important;} .ts-props .ts-search input:focus{border-color:var(--aobo-accent) !important; box-shadow:0 0 0 2px rgba(37,99,235,.12) !important;} .ts-search::before{content:\"\";position:absolute;left:.7em;top:50%;transform:translateY(-50%); width:13px;height:13px;background:var(--aobo-muted); -webkit-mask:url(\"data:image\/svg+xml;utf8,<svg xmlns='http:\/\/www.w3.org\/2000\/svg' viewBox='0 0 24 24' fill='none' stroke='black' stroke-width='2'><circle cx='11' cy='11' r='8'\/><path d='m21 21-4.3-4.3'\/><\/svg>\") center\/contain no-repeat; mask:url(\"data:image\/svg+xml;utf8,<svg xmlns='http:\/\/www.w3.org\/2000\/svg' viewBox='0 0 24 24' fill='none' stroke='black' stroke-width='2'><circle cx='11' cy='11' r='8'\/><path d='m21 21-4.3-4.3'\/><\/svg>\") center\/contain no-repeat;} .ts-chips{display:flex;flex-wrap:wrap;gap:6px;} .ts-props .ts-chip{border:1px solid var(--aobo-border-dark) !important;background:#fff !important; color:var(--aobo-text) !important;border-radius:999px !important;padding:.4em .9em !important; font-size:.8em !important;font-weight:600 !important;cursor:pointer !important;transition:all .15s !important;} .ts-props .ts-chip:hover{background:var(--aobo-hover) !important;border-color:var(--aobo-accent) !important;} .ts-props .ts-chip.on{background:var(--aobo-accent) !important;border-color:var(--aobo-accent) !important;color:#fff !important;} .ts-count{font-size:.8em;color:var(--aobo-muted);margin-left:auto;white-space:nowrap;} \/* Table *\/ .ts-table-wrap{overflow-x:auto;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius); background:#fff;box-shadow:0 1px 2px rgba(16,24,40,.04);} table.ts-table{border-collapse:collapse;width:100%;min-width:880px;font-size:.88em;} .ts-table thead th{position:sticky;top:0;z-index:2;background:var(--aobo-accent-dark);color:#fff; border-bottom:0;border-right:1px solid rgba(255,255,255,.1);text-align:center;padding:.6em .7em; font-size:.82em;font-weight:600;text-transform:none;letter-spacing:.02em;cursor:pointer; white-space:nowrap;user-select:none;} .ts-table thead th:last-child{border-right:0;} .ts-table thead th .ts-arr{color:#ffd166;font-weight:700;margin-left:3px;} .ts-table tbody td{padding:.55em .7em;border-bottom:1px solid var(--aobo-border);text-align:center; vertical-align:middle;white-space:nowrap;} .ts-table tbody tr:nth-child(even){background:var(--aobo-stripe);} .ts-table tbody tr:hover{background:var(--aobo-hover);} .ts-table tbody tr.ts-group td{background:#e8ecf1;font-weight:700;font-size:.78em;letter-spacing:.05em; text-transform:uppercase;color:#3c4043;padding:.55em .7em;border-bottom:1px solid var(--aobo-border); text-align:left;} .ts-table tbody tr:not(.ts-group).ts-hide{display:none;} td.ts-grade{font-weight:700;font-size:.95em;text-align:left;white-space:nowrap;color:var(--aobo-text);} .ts-meter{display:inline-flex;align-items:center;gap:7px;} .ts-meter i{display:inline-block;width:44px;height:6px;border-radius:3px;background:var(--aobo-fill);overflow:hidden;} .ts-meter i b{display:block;height:100%;border-radius:3px;background:linear-gradient(90deg,#4d94ff,var(--aobo-accent));} .ts-meter span{font-size:.9em;font-weight:600;min-width:14px;} .ts-hr{font-variant-numeric:tabular-nums;font-weight:500;} .ts-num{font-variant-numeric:tabular-nums;} .ts-sup{font-size:9px;color:var(--aobo-accent);vertical-align:super;line-height:0;} \/* Footnotes *\/ .ts-notes-list{margin:1.2em 0 0;background:#fff;border:1px solid var(--aobo-border); border-left:3px solid var(--aobo-accent);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0; padding:1em 1.2em 1em 2.2em;font-size:.82em;color:var(--aobo-muted);line-height:1.7;} .ts-notes-list li{margin-bottom:.3em;} .ts-notes-list sup{color:var(--aobo-accent);font-size:10px;} \/* Figure *\/ .ts-fig{margin:1.2em 0 0;background:#fff;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);padding:1em;} .ts-fig img{display:block;width:100%;height:auto;border-radius:6px;} .ts-fig figcaption{font-size:.8em;color:var(--aobo-muted);margin-top:.6em;line-height:1.6;} .ts-fig figcaption b{color:var(--aobo-text);} \/* Info cards *\/ .ts-grid{display:grid;grid-template-columns:repeat(auto-fit,minmax(250px,1fr));gap:14px;margin-top:1.2em;} .ts-grid .ts-card{background:#fff;border:1px solid var(--aobo-border);border-left:3px solid var(--aobo-accent); border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;padding:1em 1.2em;} .ts-grid h2{font-size:1em;margin:0 0 .4em;color:var(--aobo-text);} .ts-grid p{font-size:.82em;color:var(--aobo-muted);margin:0;line-height:1.7;} .ts-grid p b{color:var(--aobo-text);font-weight:600;} \/* Disclaimer *\/ .ts-disclaimer{margin-top:1.2em;background:#fff;border:1px solid var(--aobo-border); border-left:3px solid var(--aobo-accent);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0; padding:1em 1.2em;} .ts-disclaimer h3{margin:0 0 .5em;font-size:.95em;color:var(--aobo-text);display:flex;align-items:center;gap:6px;} .ts-disclaimer h3::before{content:\"\\2139\";font-size:1em;color:var(--aobo-accent);} .ts-disclaimer p{margin:0 0 .5em;max-width:none;color:var(--aobo-muted);line-height:1.7;} .ts-disclaimer p:last-child{margin-bottom:0;} \/* Empty \/ source *\/ .ts-empty{display:none;text-align:center;color:var(--aobo-muted);padding:2em 1em;font-size:.9em;} .ts-empty.show{display:block;} .ts-source{margin-top:.8em;color:var(--aobo-muted);font-size:.82em;line-height:1.58;} @media (max-width:860px){ .ts-hero-top,.ts-tool-area{padding:1em;} .ts-controls{flex-direction:column;align-items:stretch;} .ts-search{max-width:none;} .ts-count{margin-left:0;} .ts-hero h1{font-size:1.5rem;} } @media (max-width:520px){ .ts-hero-top,.ts-tool-area{padding:.8em;} table.ts-table{font-size:.82em;} .ts-table thead th,.ts-table tbody td{padding:.4em .4em;} } table.ts-table thead th{cursor:default;} table.ts-table td.ts-grade{font-weight:700;} table.ts-table td.ts-type{white-space:normal;text-align:left;font-size:.92em;color:#555;min-width:150px;} table.ts-table td.ts-long{white-space:normal;text-align:left;vertical-align:top;font-size:.92em;color:#444; min-width:260px;line-height:1.55;} table.ts-table td.ts-safe{white-space:normal;text-align:left;vertical-align:top;} table.ts-table tbody tr:hover{background:var(--aobo-hover);} table.ts-table tbody tr.ts-group:hover td{background:#e8ecf1;} .ts-sec{margin:1.8em 0 .5em;font-size:1.02em;color:var(--aobo-text);font-weight:700;} .ts-sec span{display:block;font-size:.8em;font-weight:400;color:var(--aobo-muted);margin-top:.15em;line-height:1.6;} .ts-table-wrap{margin-top:.6em;} .ts-tcap{margin:.5em 0 0;font-size:.78em;color:var(--aobo-muted);line-height:1.6;} .ts-props a{color:var(--aobo-blue) !important;text-decoration:none !important;} .ts-props a:hover{text-decoration:underline !important;} .ts-rel{margin-top:1.2em;background:#fff;border:1px solid var(--aobo-border); border-left:3px solid var(--aobo-blue);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;padding:1em 1.2em;} .ts-rel h3{margin:0 0 .5em;font-size:.95em;color:var(--aobo-text);} .ts-rel p{margin:0;font-size:.85em;line-height:1.9;color:var(--aobo-muted);} .ts-rel p a{font-weight:600;} .aobo-ht-ref.ts-props table.ts-table.wraphead thead th{white-space:normal;line-height:1.25;} .aobo-ht-ref.ts-props table.ts-table.wraphead tbody td{white-space:nowrap !important;}\n<\/style> <style id=\"aobo-dl-css\">\n.aobo-ht-ref.ts-props .ts-dl{display:flex !important;flex-wrap:wrap;align-items:center;gap:1em; background:var(--aobo-stripe) !important;border:1px solid var(--aobo-border) !important; border-radius:var(--aobo-radius) !important;padding:1.1em 1.3em !important;margin:1.5em 0 !important;}\n.aobo-ht-ref.ts-props .ts-dl-txt{flex:1 1 340px;font-size:.95em;color:var(--aobo-text) !important;line-height:1.55;}\n.aobo-ht-ref.ts-props .ts-dl-txt strong{display:block;font-weight:700 !important;margin-bottom:.2em;color:var(--aobo-text) !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn{display:inline-flex !important;align-items:center;gap:.5em; background:var(--aobo-blue) !important;color:#fff !important;border:1px solid var(--aobo-blue) !important; border-radius:var(--aobo-radius-sm) !important;padding:.75em 1.35em !important;font-size:.95em !important; font-weight:600 !important;text-decoration:none !important;white-space:nowrap;box-shadow:none !important; line-height:1.3 !important;text-transform:none !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn:hover,.aobo-ht-ref.ts-props a.ts-dl-btn:focus{background:var(--aobo-blue-dark) !important; border-color:var(--aobo-blue-dark) !important;color:#fff !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn svg{width:1.05em;height:1.05em;fill:none;stroke:currentColor;stroke-width:2;flex:0 0 auto;}\n@media (max-width:640px){.aobo-ht-ref.ts-props a.ts-dl-btn{width:100%;justify-content:center;}}\n<\/style> <style id=\"aobo-ds\">\n.entry-content[class]{--ds-font-body: Lora,serif;--ds-font-head: Lato,sans-serif;--ds-blue: #0c56d0;--ds-blue-deep: #082d6f;--ds-blue-dark: #073b91;--ds-blue-soft: #eaf2ff;--ds-blue-pale: #f7fbff;--ds-border: #d7e5fb;--ds-border-soft: #e8eef8;--ds-text: #203044;--ds-muted: #617087;--ds-orange: #f59b23;--ds-shadow: 0 18px 45px rgba(12,86,208,0.10);--ds-shadow-sm: 0 12px 32px rgba(12,86,208,0.07);font-family: var(--ds-font-body);line-height: 1.7;-webkit-text-size-adjust: 100%;box-sizing: border-box}.entry-content[class] *,.entry-content[class] *::before,.entry-content[class] *::after{box-sizing: border-box}.entry-content[class] h1{font-family: var(--ds-font-head) !important;font-size: clamp(24px,4vw,min(50px,var(--h1-max,50px))) !important;line-height: 1.08 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 0 0 16px !important}.entry-content[class] h2{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 44px 0 16px !important}.entry-content[class] h3{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.3 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 30px 0 12px !important}.entry-content[class] h4{font-family: var(--ds-font-head) !important;font-size: 19px !important;line-height: 1.35 !important;letter-spacing: 0 !important;font-weight: 700 !important;margin: 24px 0 10px !important}.entry-content[class] p,.entry-content[class] li,.entry-content[class] dd,.entry-content[class] dt{font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important}.entry-content[class] figcaption,.entry-content[class] small,.entry-content[class] .aobo-figure figcaption{font-size: 15px !important;line-height: 1.6 !important}.entry-content[class] table{width: 100%;border-collapse: collapse;background: #ffffff}.entry-content[class] table th,.entry-content[class] table thead th,.entry-content[class] table thead td{background: var(--ds-blue-soft) !important;color: var(--ds-blue-deep) !important;font-family: var(--ds-font-head) !important;font-size: 15px !important;font-weight: 700 !important;line-height: 1.45 !important;text-align: center !important;text-transform: none !important;letter-spacing: 0 !important;padding: 14px 16px !important;border: 0 !important;border-bottom: 1px solid var(--ds-border) !important;vertical-align: top !important;position: static !important}.entry-content[class] table td{font-family: var(--ds-font-body) !important;font-size: 15px !important;line-height: 1.55 !important;padding: 14px 16px !important;border: 0;border-bottom: 1px solid var(--ds-border-soft) !important;vertical-align: top !important;white-space: normal !important;text-align: center !important}.entry-content[class] table tbody tr:last-child td{border-bottom: 0 !important}.entry-content[class] table th.ds-text,.entry-content[class] table td.ds-text{text-align: left !important}.entry-content[class] table tbody tr:nth-child(even){background: #fafcff !important}.entry-content[class] table tbody tr:hover{background: #f2f7ff !important}.entry-content[class] table tbody td:first-child{color: var(--ds-blue-deep);font-weight: 700}.entry-content[class] .aobo-table-wrap,.entry-content[class] .ts-table-wrap{overflow-x: auto;margin: 22px 0 28px;border: 1px solid var(--ds-border);border-radius: 18px;box-shadow: var(--ds-shadow-sm);background: #ffffff}.entry-content[class] h1,.entry-content[class] h2,.entry-content[class] h3,.entry-content[class] h4{color: var(--ds-blue-deep)}.entry-content[class] p,.entry-content[class] li{color: var(--ds-text)}.entry-content[class] a{color: var(--ds-blue);font-weight: 700;text-decoration: none}.entry-content[class] a:hover,.entry-content[class] a:focus{color: var(--ds-orange)}.entry-content[class] .aobo-final-cta h1,.entry-content[class] .aobo-final-cta h2,.entry-content[class] .aobo-final-cta h3,.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-cta h1,.entry-content[class] .aobo-cta h2,.entry-content[class] .aobo-cta h3,.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-cta-buttons,.entry-content[class] .aobo-cta-buttons *,.entry-content[class] .aobo-esr .stat-band h2,.entry-content[class] .aobo-esr .stat-band h3,.entry-content[class] .aobo-esr .stat-band p,.entry-content[class] .aobo-esr .closing h2,.entry-content[class] .aobo-esr .closing h3,.entry-content[class] .aobo-esr .closing p,.entry-content[class] .footcta h2,.entry-content[class] .footcta h3,.entry-content[class] .footcta p,.entry-content[class] .bg-dark h2,.entry-content[class] .bg-dark h3,.entry-content[class] .bg-dark p,.entry-content[class] .ht-header h2,.entry-content[class] .ht-header h3,.entry-content[class] .ts-cta h2,.entry-content[class] .ts-cta h3,.entry-content[class] .aobo-sup .stats h2,.entry-content[class] .aobo-sup .stats h3,.entry-content[class] .aobo-sup .stats p,.entry-content[class] .aobo-sup .cta h2,.entry-content[class] .aobo-sup .cta h3,.entry-content[class] .aobo-sup .cta p{color: inherit}.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-sup .cta p{color: rgba(255,255,255,0.92)}.entry-content[class] .has-ast-global-color-0-background-color,.entry-content[class] .has-ast-global-color-0-background-color *,.entry-content[class] .contact-container,.entry-content[class] .contact-container *{color: #ffffff !important}.entry-content[class] .has-ast-global-color-0-background-color .label-text,.entry-content[class] .has-ast-global-color-0-background-color .label-text *,.entry-content[class] .contact-container .label-text{color: rgba(255,255,255,0.72) !important}.entry-content[class] .aobo-cta h1,.entry-content[class] .aobo-cta h2,.entry-content[class] .aobo-cta h3,.entry-content[class] .aobo-cta h4,.entry-content[class] .cta h1,.entry-content[class] .cta h2,.entry-content[class] .cta h3,.entry-content[class] .cta h4,.entry-content[class] .aobo-final-cta h1,.entry-content[class] .aobo-final-cta h2,.entry-content[class] .aobo-final-cta h3,.entry-content[class] .aobo-final-cta h4{color: #ffffff !important}.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-cta li,.entry-content[class] .cta p,.entry-content[class] .cta li,.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-final-cta li{color: rgba(255,255,255,0.93) !important}.entry-content[class] .aobo-cta p a,.entry-content[class] .aobo-cta li a,.entry-content[class] .cta p a,.entry-content[class] .cta li a,.entry-content[class] .aobo-final-cta p a,.entry-content[class] .aobo-final-cta li a{color: #ffffff !important;text-decoration: underline}.entry-content[class] .aobo-btn-inquiry{color: #ffffff !important}.entry-content[class] .aobo-cta .aobo-btn-inquiry,.entry-content[class] .aobo-final-cta .aobo-btn-inquiry{color: var(--ds-blue) !important}.entry-content[class] .aobo-wrap,.entry-content[class] .aobo-article{max-width: 1180px;margin: 0 auto;padding: 0}.entry-content[class] img{max-width: 100%;height: auto}.entry-content[class] figure{margin: 26px auto 34px;max-width: 860px}.entry-content[class] figure img{display: block;width: 100%;border: 1px solid var(--ds-border);border-radius: 18px;box-shadow: var(--ds-shadow-sm);background: #ffffff}.entry-content[class] .aobo-hero{background: linear-gradient(135deg,#ffffff 0%,#f7fbff 56%,#eaf2ff 100%);border: 1px solid var(--ds-border);border-radius: 28px;padding: 42px 38px;margin-bottom: 24px;box-shadow: var(--ds-shadow);overflow: hidden;position: relative}.entry-content[class] .aobo-hero::after{content: \"\";position: absolute;right: -90px;top: -90px;width: 260px;height: 260px;border-radius: 50%;background: rgba(12,86,208,0.08)}.entry-content[class] .aobo-hero h1,.entry-content[class] .aobo-hero p{position: relative;z-index: 2}.entry-content[class] .aobo-note-box{margin: 34px 0;padding: 22px 24px;border: 1px solid var(--ds-border);border-left: 5px solid var(--ds-orange);border-radius: 16px;background: #fbfdff}.entry-content[class] .aobo-note-box p{margin: 0 0 14px;color: var(--ds-muted) !important;font-style: italic}.entry-content[class] .aobo-note-box p:last-child{margin-bottom: 0}.entry-content[class] .aobo-btn{display: inline-flex;align-items: center;justify-content: center;min-height: 42px;padding: 10px 16px;border-radius: 999px;text-align: center;text-decoration: none;font-family: var(--ds-font-head) !important;font-weight: 700;font-size: 14px !important;line-height: 1.2;transition: all 0.2s ease;cursor: pointer;white-space: nowrap}.entry-content[class] .aobo-btn-primary{background: var(--ds-blue);border: 1px solid var(--ds-blue);color: #ffffff !important}.entry-content[class] .aobo-btn-secondary{background: #ffffff;border: 1px solid var(--ds-border);color: var(--ds-blue) !important}.entry-content[class] .aobo-btn:hover{transform: translateY(-1px)}.entry-content[class] .aobo-supply-actions{display: flex;flex-wrap: wrap;gap: 12px;margin-top: 18px}.entry-content[class] .aobo-supply-actions .aobo-btn{min-width: 190px}.entry-content[class] .aobo-final-cta{margin-top: 34px;padding: 34px;border-radius: 28px;background: linear-gradient(135deg,#073b91 0%,#0c56d0 100%);box-shadow: 0 18px 45px rgba(12,86,208,0.20);display: flex;align-items: center;justify-content: space-between;gap: 20px;flex-wrap: wrap}.entry-content[class] .aobo-final-cta h2{margin: 0 0 12px !important;font-size: 26px !important;color: #ffffff !important}.entry-content[class] .aobo-final-cta p{margin: 0}.entry-content[class] .aobo-final-cta .aobo-btn-primary{background: #ffffff;border-color: #ffffff;color: var(--ds-blue) !important}.entry-content[class] .aobo-final-cta .aobo-btn-secondary{background: transparent;border-color: rgba(255,255,255,0.75);color: #ffffff !important}.entry-content[class] .ts-hero{background: transparent !important;border: 0 !important;border-radius: 0 !important;box-shadow: none !important}.entry-content[class] .ts-hero-top{background: linear-gradient(135deg,#ffffff 0%,#f7fbff 56%,#eaf2ff 100%) !important;border: 1px solid var(--ds-border) !important;border-radius: 28px !important;padding: 42px 38px !important;margin: 0 0 24px !important;box-shadow: var(--ds-shadow) !important;position: relative;overflow: hidden;text-align: left !important}.entry-content[class] .ts-hero-top h1,.entry-content[class] .ts-hero-top p,.entry-content[class] .ts-hero h1{text-align: left !important}.entry-content[class] .ts-hero-top p{max-width: none !important;margin: 0 0 12px !important}.entry-content[class] .ts-tool-area{padding: 0 !important}.entry-content[class] .ts-sec{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 44px 0 16px !important}.entry-content[class] .ts-sec > span{display: block !important;font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important;font-weight: 400 !important;color: var(--ds-text) !important;margin: 0 0 16px !important}.entry-content[class] .ts-kicker{display: inline-flex !important;align-items: center;gap: 7px;margin: 0 0 14px !important;padding: 6px 14px !important;border: 1px solid var(--ds-border) !important;border-radius: 999px !important;background: #ffffff !important;color: var(--ds-blue) !important;font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important;letter-spacing: 0 !important;text-transform: none !important}.entry-content[class] .ts-p,.entry-content[class] .card-desc,.entry-content[class] .aobo-strip-intro,.entry-content[class] .schema-faq-answer{font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important;font-weight: 400 !important}.entry-content[class] .lead,.entry-content[class] .fund-lead{font-family: var(--ds-font-body) !important;font-size: 19px !important;line-height: 1.65 !important;font-weight: 400 !important}.entry-content[class] .ts-h2{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 44px 0 16px !important}.entry-content[class] .ts-h3{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.3 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 30px 0 12px !important}.entry-content[class] .card-grade{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.25 !important;font-weight: 700 !important}.entry-content[class] .schema-faq-question{font-family: var(--ds-font-head) !important;font-size: 19px !important;line-height: 1.4 !important;font-weight: 700 !important;color: var(--ds-blue-deep) !important}.entry-content[class] .ts-source,.entry-content[class] .ts-hint,.entry-content[class] .ts-placeholder,.entry-content[class] .ht-spec-label,.entry-content[class] .ht-spec-value,.entry-content[class] .ht-step-indicator,.entry-content[class] .ht-badge,.entry-content[class] .idx,.entry-content[class] .xlink,.entry-content[class] .cat-note,.entry-content[class] .aobo-card-note,.entry-content[class] .card-desig,.entry-content[class] .k,.entry-content[class] .v,.entry-content[class] .note,.entry-content[class] .aobo-note{font-family: var(--ds-font-head) !important;font-size: 15px !important;line-height: 1.6 !important;font-weight: 400 !important}.entry-content[class] .ht-spec-label,.entry-content[class] .idx,.entry-content[class] .k{font-weight: 700 !important}.entry-content[class] .aobo-note,.entry-content[class] .note{font-family: var(--ds-font-body) !important;color: var(--ds-muted) !important}.entry-content[class] .chip{font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important}.entry-content[class] .kicker,.entry-content[class] .eyebrow,.entry-content[class] .aobo-eyebrow{display: inline-flex !important;align-items: center;gap: 7px;margin: 0 0 14px !important;padding: 6px 14px !important;border: 1px solid var(--ds-border) !important;border-radius: 999px !important;background: #ffffff !important;color: var(--ds-blue) !important;font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important;letter-spacing: 0 !important;text-transform: none !important}@media (max-width: 760px){.entry-content[class] h1{font-size: clamp(22px,6.4vw,min(34px,var(--h1-max,34px))) !important}.entry-content[class] h2{font-size: 25px !important}.entry-content[class] h3{font-size: 20px !important}.entry-content[class] h4{font-size: 17px !important}.entry-content[class] p,.entry-content[class] li{font-size: 16px !important}.entry-content[class] table th,.entry-content[class] table td{font-size: 14px !important;padding: 11px 12px !important}.entry-content[class] .aobo-hero{padding: 30px 22px}.entry-content[class] .aobo-final-cta{padding: 26px 22px}.entry-content[class] .aobo-final-cta .aobo-btn{width: 100%}}\n<\/style>\n<section class=\"aobo-ht-ref ts-props\">\n<div class=\"aobo-wrap\"> <div class=\"ts-hero\">\n<div class=\"ts-hero-top\">\n<div class=\"ts-kicker\"><span><\/span>Tool Steel | Cold Work | Heat Treating<\/div>\n<h1 style=\"--h1-max:44px\">Cold Work Tool Steel Heat Treatment<\/h1>\n<p>Cold work tool steels split into three groups by the way they are quenched, and the group decides almost everything else about the cycle. The oil hardening grades O1, O2, O6 and O7 are quenched in oil and tempered low. The medium-alloy air hardening grades of the A group and the high-carbon high-chromium grades of the D group harden in still air, so their quenching is really a question of how much air, and their tempering goes far higher because they soften slowly. This page carries the hardenability data that decides whether still air is enough, the measured austenitizing procedures for two D2 die inserts, and the tempering response curves for both families.<\/p>\n<\/div>\n<\/div> <div class=\"ts-tool-area\"> <h2 class=\"ts-h2\">Whether still air will do the job<\/h2>\n<p class=\"ts-p\">Every steel in the A group and every steel in the D group except D3 reaches full hardness by cooling in still air, as long as the section is not extremely large. How large is too large is the whole question, and the table below answers it for the grades the source tested. A section that will not harden through in still air does not need a different steel. It needs a faster cool, and the source lists the steps in order of severity, from still air with no artificial circulation, through fan air, through a high-pressure air blast, then an oil quench stopped while the steel is still above a dull red and finished in air, and finally a conventional oil quench. Each step down that list buys hardness at the cost of distortion, so the first step that works is the one to use.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:900px;\">\n<thead><tr><th rowspan=\"2\">Steel<\/th><th colspan=\"2\">Centre hardening<\/th><th colspan=\"2\">Surface hardening<\/th><\/tr><tr><th>Size of section that fully hardens at the centre<\/th><th>Hardness, HRC<\/th><th>Size of section that fully hardens at the surface<\/th><th>Hardness, HRC<\/th><\/tr><\/thead>\n<tbody>\n<tr><td class=\"ts-grade\">A2, A4<\/td><td class=\"ts-num\">75 mm (3 in.) diam<\/td><td class=\"ts-num\">59-61<\/td><td class=\"ts-num\">100 mm (4 in.) diam<\/td><td class=\"ts-num\">59-61<\/td><\/tr>\n<tr><td class=\"ts-grade\">A5<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">100 mm (4 in.) diam<\/td><td class=\"ts-num\">62-63<\/td><\/tr>\n<tr><td class=\"ts-grade\">A6<\/td><td class=\"ts-num\">180 mm (7 in.) cube<\/td><td class=\"ts-num\">59-60<\/td><td class=\"ts-num\">180 mm (7 in.) cube<\/td><td class=\"ts-num\">60-61<\/td><\/tr>\n<tr><td class=\"ts-grade\">D1, D2, D5<\/td><td class=\"ts-num\">100 mm (4 in.) cube<\/td><td class=\"ts-num\">60-61<\/td><td class=\"ts-num\">125 &times; 125 &times; 255 mm (5 &times; 5 &times; 10 in.)<\/td><td class=\"ts-num\">61-62<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 8 of Heat Treating of Specific Classes of Tool Steels. Section sizes that reach full hardness when the steel is cooled in still air, read at the centre and at the surface of the section.<\/em><\/p> <h2 class=\"ts-h2\">Austenitizing the A and D steels<\/h2>\n<p class=\"ts-p\">These grades are preheated before austenitizing, because preheating cuts the distortion that comes from uneven dimensional change during the rise to temperature. Types A4, A5, A6 and A10 are austenitized low enough that preheating can often be dropped when the tool goes into a furnace rather than a liquid bath. A2, A3, A7, A8, A9 and all the D grades are preheated at 790 to 815 &deg;C (1450 to 1500 &deg;F), and at that temperature a liquid bath or a protective atmosphere is required to stop scale and decarburization.<\/p>\n<p class=\"ts-p\">Above 650 &deg;C (1200 &deg;F) the surface has to be protected. Endothermic gas from a generator is the usual choice and it is controlled by dew point. Dry dissociated ammonia at a dew point of -50 &deg;C (-60 &deg;F) and dry hydrogen at -75 &deg;C (-100 &deg;F) are used where no discoloration at all is acceptable. Vacuum suits the A and D steels particularly well, because their air hardening response lets them cool slowly enough to be quenched in the same furnace. The hold at the austenitizing temperature has to be long enough for the carbides to dissolve, since that is what sets the hardness ceiling, but an austenitizing temperature pushed higher than it needs to be raises the retained austenite, and retained austenite that is corrected afterwards by repeated tempering or a subzero cool is a correction that should never have been needed. The table below shows how two real parts were run, one in a salt bath and one in an endothermic atmosphere furnace.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:820px;\">\n<thead><tr><th>Part and process<\/th><th>Procedure<\/th><\/tr><\/thead>\n<tbody>\n<tr><td class=\" colspan=\"2\" class=\"ts-type\"\">Bending die inserts (a)<\/td><\/tr>\n<tr><td>Salt bath (b)<\/td><td>Preheat in air furnace at 650 &deg;C (1200 &deg;F) for 1 1\/2 h (c), austenitize at 1010 &deg;C (1850 &deg;F) for 35 min (c), air cool, remove salt<\/td><\/tr>\n<tr><td>Endothermic atmosphere (d)<\/td><td>Charge directly into furnace at 705 &deg;C (1300 &deg;F) and preheat for 1 1\/2 h (c), austenitize at 1010 &deg;C (1850 &deg;F) for 2 h, air cool (c)<\/td><\/tr>\n<tr><td class=\" colspan=\"2\" class=\"ts-type\"\">Trim die inserts (e)<\/td><\/tr>\n<tr><td>Salt bath (b)<\/td><td>Preheat in air furnace at 650 &deg;C (1200 &deg;F), 4 h (c), then in salt bath at 845 &deg;C (1550 &deg;F), 1 h (c) (f), austenitize at 1010 &deg;C (1850 &deg;F) for 1 h (c), air cool (c), remove salt<\/td><\/tr>\n<tr><td>Endothermic atmosphere (d)<\/td><td>Charge directly into furnace at 705 &deg;C (1300 &deg;F) and preheat for 4 h (c), raise furnace temperature and austenitize at 1010 &deg;C (1850 &deg;F) for 4 h, air cool (c)<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 7 of Heat Treating of Specific Classes of Tool Steels. (a) After austenitizing, inserts 200 by 305 by 38 mm (8 by 12 by 1 1\/2 in.) were double tempered, 2 h at 510 &deg;C (950 &deg;F), air cool, repeated, and then nitrided for 48 h at 510 &deg;C (950 &deg;F). (b) The salt bath furnace was an immersed-electrode type, 380 by 760 by 915 mm (15 by 30 by 36 in.) deep. (c) Manual loading requires 1 1\/2 min per piece. (d) The furnace was a radiant-tube type, 610 by 915 by 455 mm (24 by 36 by 18 in.) high. (e) After austenitizing, the die inserts were double tempered, 4 h at 190 &deg;C (375 &deg;F), air cool, repeated. (f) The second preheat was necessary because of the faster heating rate of the salt bath.<\/em><\/p> <h2 class=\"ts-h2\">Tempering the oil hardening steels<\/h2>\n<p class=\"ts-p\">The O grades soften quickly once the tempering temperature climbs, and the curves below show four of them side by side. The austenitizing temperature matters as much as the tempering temperature, and it moves the whole curve rather than one region of it. Conventional O grade tools are rarely given a second temper or a subzero cool. The exception is a tool where dimensional stability is the whole point, such as a gauge, and for those the work is cooled below 65 &deg;C (150 &deg;F) before each retemper and a subzero cool to -75 &deg;C (-100 &deg;F) or lower is worth adding.<\/p>\n<figure>\n<img src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png\" alt=\"Hardness against tempering temperature for oil hardening cold work tool steels O1, O2, O6 and O7\" width=\"968\" height=\"676\" loading=\"lazy\" decoding=\"async\">\n<figcaption>Fig. 1. Hardness as a function of tempering temperature for the oil hardening cold work tool steels O1, O2, O6 and O7. Reproduced from the source figure. O1, O2 and O6 were oil quenched after austenitizing at the temperature marked on each panel. For O7, the large uniform sections were water quenched after 800 to 830 &deg;C (1475 to 1525 &deg;F) and the other sections were oil quenched after 830 to 870 &deg;C (1525 to 1600 &deg;F). The tempering time was 1 h in every case.<\/figcaption>\n<\/figure> <h2 class=\"ts-h2\">Tempering the air hardening and high chromium steels<\/h2>\n<p class=\"ts-p\">The A and D grades hold their hardness much further up the temperature scale than the O grades, and that is what makes them useful in a die that runs warm. Tempering usually starts when the part has cooled to about 50 to 65 &deg;C (120 to 150 &deg;F) rather than to room temperature, because cooling all the way down first raises the risk of cracking without changing the outcome much. These steels do hold some austenite at that point, and the usual answer is a double or a triple temper rather than a subzero cool. A minimum tempering temperature of 205 &deg;C (400 &deg;F) is a common requirement for A2, A7 and the D steels, and temperatures up to 550 &deg;C (1025 &deg;F) are normal, with higher temperatures used for special requirements. The two figures below show the shape of the response for both families.<\/p>\n<figure>\n<img src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-7-air-hardening-tempering.png\" alt=\"Effect of tempering temperature on hardness of medium alloy air hardening tool steels\" width=\"964\" height=\"467\" loading=\"lazy\" decoding=\"async\">\n<figcaption>Fig. 2. Effect of tempering temperature on the hardness of medium-alloy air hardening tool steels. Reproduced from the source figure. The left panel is A2 and the right panel groups the other A grades, with each set of points marked by its austenitizing temperature.<\/figcaption>\n<\/figure>\n<figure>\n<img src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-8-d2-d3-tempering.png\" alt=\"Relation between tempering temperature and hardness for D2 and D3 tool steels\" width=\"968\" height=\"467\" loading=\"lazy\" decoding=\"async\">\n<figcaption>Fig. 3. Relation between tempering temperature and hardness for D2 and D3 tool steels. Reproduced from the source figure. Each panel shows the secondary hardening peak that these high-chromium grades develop, and the position of that peak moves with the austenitizing temperature, so the same steel tempered at the same temperature gives two different hardnesses on two different hardening cycles.<\/figcaption>\n<\/figure> <h2 class=\"ts-h2\">What to check before release<\/h2>\n<p class=\"ts-p\">Two things decide whether a cold work tool comes out of a furnace the way the route card says it will. The first is whether the section actually hardened through, which for an air hardening grade means checking the core and not the surface, because the surface will read hard on a section that never hardened at the centre. The second is the austenitizing temperature, because it sets both the hardness ceiling and the position of the secondary hardening peak, and a small error there shows up as a large error in the finished hardness. Check the first article at the core, against the as-quenched hardness the steel is supposed to reach, before the cycle is released.<\/p> <p class=\"ts-source\">Source: ASM Handbook, Volume 4, Heat Treating, ASM International, 1991.<\/p> <\/div><\/div><\/div><\/section>\n","protected":false},"excerpt":{"rendered":"<p>Tool Steel | Cold Work | Heat Treating Cold Work Tool Steel Heat Treatment Cold work tool steels split into three groups by the way they are quenched, and the group decides almost everything else about the cycle. The oil hardening grades O1, O2, O6 and O7 are quenched in oil and tempered low. The [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20886","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.6 (Yoast SEO v28.6) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Cold Work Tool Steel Heat Treating, Hardenability and Tempering<\/title>\n<meta name=\"description\" content=\"Still air hardenability of the A and D cold work tool steels, measured austenitizing procedures for D2 die inserts, and tempering response curves for the O, A and D groups.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/es\/cold-work-tool-steel-heat-treatment\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Cold Work Tool Steel Heat Treatment\" \/>\n<meta property=\"og:description\" content=\"Still air hardenability of the A and D cold work tool steels, measured austenitizing procedures for D2 die inserts, and tempering response curves for the O, A and D groups.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/es\/cold-work-tool-steel-heat-treatment\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-06T23:08:25+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"7 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Cold Work Tool Steel Heat Treatment\",\"datePublished\":\"2026-10-03T23:59:09+00:00\",\"dateModified\":\"2026-10-06T23:08:25+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/\"},\"wordCount\":1475,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png\",\"inLanguage\":\"es\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/\",\"name\":\"Cold Work Tool Steel Heat Treating, Hardenability and Tempering\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png\",\"datePublished\":\"2026-10-03T23:59:09+00:00\",\"dateModified\":\"2026-10-06T23:08:25+00:00\",\"description\":\"Still air hardenability of the A and D cold work tool steels, measured austenitizing procedures for D2 die inserts, and tempering response curves for the O, A and D groups.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cold-work-tool-steel-heat-treatment\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Cold Work Tool Steel Heat Treatment\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/es\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Cold Work Tool Steel Heat Treating, Hardenability and Tempering","description":"Still air hardenability of the A and D cold work tool steels, measured austenitizing procedures for D2 die inserts, and tempering response curves for the O, A and D groups.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/es\/cold-work-tool-steel-heat-treatment\/","og_locale":"es_ES","og_type":"article","og_title":"Cold Work Tool Steel Heat Treatment","og_description":"Still air hardenability of the A and D cold work tool steels, measured austenitizing procedures for D2 die inserts, and tempering response curves for the O, A and D groups.","og_url":"https:\/\/aobosteel.com\/es\/cold-work-tool-steel-heat-treatment\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-06T23:08:25+00:00","og_image":[{"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_misc":{"Tiempo de lectura":"7 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Cold Work Tool Steel Heat Treatment","datePublished":"2026-10-03T23:59:09+00:00","dateModified":"2026-10-06T23:08:25+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/"},"wordCount":1475,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png","inLanguage":"es"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/","url":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/","name":"Cold Work Tool Steel Heat Treating, Hardenability and Tempering","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png","datePublished":"2026-10-03T23:59:09+00:00","dateModified":"2026-10-06T23:08:25+00:00","description":"Still air hardenability of the A and D cold work tool steels, measured austenitizing procedures for D2 die inserts, and tempering response curves for the O, A and D groups.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/"]}]},{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Cold-Work-Tool-Steel-Heat-Treatment-fig-6-o-steels-tempering.png"},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/cold-work-tool-steel-heat-treatment\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Cold Work Tool Steel Heat Treatment"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tool Steel | Cold Work | Heat Treating Cold Work Tool Steel Heat Treatment Cold work tool steels split into three groups by the way they are quenched, and the group decides almost everything else about the cycle. The oil hardening grades O1, O2, O6 and O7 are quenched in oil and tempered low. The&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tool Steel | Cold Work | Heat Treating Cold Work Tool Steel Heat Treatment Cold work tool steels split into three groups by the way they are quenched, and the group decides almost everything else about the cycle. The oil hardening grades O1, O2, O6 and O7 are quenched in oil and tempered low. The&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20886","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/comments?post=20886"}],"version-history":[{"count":2,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20886\/revisions"}],"predecessor-version":[{"id":21061,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20886\/revisions\/21061"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/media?parent=20886"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}