{"id":20442,"date":"2026-10-01T09:11:55","date_gmt":"2026-10-01T01:11:55","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20442"},"modified":"2026-10-16T00:40:35","modified_gmt":"2026-10-15T16:40:35","slug":"tool-steel-fracture-toughness-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/es\/tool-steel-fracture-toughness-chart\/","title":{"rendered":"Tabla de tenacidad a la fractura del acero para herramientas (K1c)"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Tabla de tenacidad a la fractura del acero para herramientas (K1c)<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">Tenacidad a la fractura en MPa ra\u00edz metro para ocho grados comunes de acero para herramientas, medida en probetas de flexi\u00f3n tomadas de tres reducciones de forja y revenidas a tres temperaturas, con la dureza a la que se ensay\u00f3 cada probeta. Un resumen de referencia de la pr\u00e1ctica publicada y no una especificaci\u00f3n de Aobo Steel.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">C\u00f3mo se obtuvieron los valores<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Cada cifra de esta p\u00e1gina proviene de un programa de laboratorio que realiz\u00f3 tres ensayos de tenacidad en paralelo sobre los mismos ocho grados, por lo que los n\u00fameros pueden compararse entre s\u00ed. Los aceros se suministraron como lingotes de 432 mm de di\u00e1metro refundidos por escoria electroconductora. Se cortaron muestras de cada grado de barra redonda de 146 a 173 mm y parte de cada una se forj\u00f3 hasta 89 mm cuadrados y 38 mm cuadrados, lo que da las tres reducciones totales de forja indicadas como 88, 95 y 99 por ciento.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">La tenacidad a la fractura se midi\u00f3 en probetas de flexi\u00f3n est\u00e1ndar de 114 mm por 25 mm por 13 mm, mecanizadas ligeramente sobredimensionadas en la dimensi\u00f3n de 25 mm, entalladas, tratadas t\u00e9rmicamente y luego mecanizadas en acabado antes del ensayo a temperatura ambiente. Se revenieron probetas duplicadas y algunas triplicadas a cada una de tres temperaturas de revenido por grado, por lo que la mayor\u00eda de las filas llevan dos valores de ensayo y las filas de H13 llevan tres. La dureza se midi\u00f3 en cada probeta despu\u00e9s del ensayo, por lo que la columna HRC es la dureza a la que se ensay\u00f3 realmente esa probeta y no una cifra nominal.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Los valores de tenacidad se dan en MPa ra\u00edz metro, escritos K1c, la tenacidad a la fractura en deformaci\u00f3n plana. La pr\u00e1ctica de austenizaci\u00f3n y el temple difieren seg\u00fan el grado y se indican en las notas de la tabla bajo cada tabla.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Tenacidad a la fractura de los grados templados en aceite (L6 y O2)<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">K1c por reducci\u00f3n de forja, tama\u00f1o de secci\u00f3n, temperatura de revenido y dureza<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Grado<\/th><th class=\"has-text-align-left\" data-align=\"left\">Reducci\u00f3n de forja<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tama\u00f1o de secci\u00f3n<\/th><th class=\"has-text-align-left\" data-align=\"left\">Temperatura de revenido<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c (MPa&radic;m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c promedio<\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.86, 18.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.19, 22.14<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">171 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.11, 25.39<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.76, 24.79<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.04, 24.86<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">171 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.53, 28.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.15, 26.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.71, 27.42<\/td><td class=\"has-text-align-left\" data-align=\"left\">26.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">171 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.12, 30.32<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.37, 17.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.31, 19.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.80, 19.84<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">62.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.82, 18.94<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.23, 20.72<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.62, 21.49<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.66, 18.37<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.77, 19.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">288 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.31, 20.32<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, Tabla II, Resultados de las pruebas de tenacidad a la fractura de AISI L6 y O2 de materiales para herramientas para moldes y troqueles (G. Krauss y H. Nordberg, eds.).<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>La reducci\u00f3n de forja es la reducci\u00f3n total desde el lingote de 432 mm. L6 se austeniz\u00f3 en sal a 830 &#176;C durante 5 minutos y se templ\u00f3 en aceite, O2 en sal a 802 &#176;C durante 5 minutos y se templ\u00f3 en aceite. Ambos valores de cada fila son resultados de ensayo individuales sobre probetas separadas y la columna de promedio es la media aritm\u00e9tica de ellos.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Tenacidad a la fractura de D3 y A6<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">K1c donde se pudo preagrietar y ensayar una probeta<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Grado<\/th><th class=\"has-text-align-left\" data-align=\"left\">Reducci\u00f3n de forja<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tama\u00f1o de secci\u00f3n<\/th><th class=\"has-text-align-left\" data-align=\"left\">Temperatura de revenido<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c (MPa&radic;m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c promedio<\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">D3<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.54, 33.67<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D3<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.76<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">55.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.81, 21.53<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.63, 21.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">173 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.34, 25.80<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.95, 20.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.63, 21.77<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">173 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.95, 23.17<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">52.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.41, 27.09<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">49.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.60, 29.46<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">49.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">173 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.06, 29.05<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">48.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, Tabla III, Resultados de las pruebas de tenacidad a la fractura de AISI D3 y A6 de materiales para herramientas para moldes y troqueles.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>D3 se agriet\u00f3 durante el preagrietado en siete de las nueve condiciones ensayadas, por lo que solo las dos condiciones de la tabla produjeron un valor v\u00e1lido y la fuente no da cifra para las dem\u00e1s. D3 se austeniz\u00f3 en sal a 968 &#176;C durante 25 minutos y se templ\u00f3 en aceite, A6 en sal a 843 &#176;C durante 25 minutos y se enfri\u00f3 al aire.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Tenacidad a la fractura de los grados de trabajo en fr\u00edo templados al aire (A2 y D2)<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">K1c por reducci\u00f3n de forja, tama\u00f1o de secci\u00f3n, temperatura de revenido y dureza<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Grado<\/th><th class=\"has-text-align-left\" data-align=\"left\">Reducci\u00f3n de forja<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tama\u00f1o de secci\u00f3n<\/th><th class=\"has-text-align-left\" data-align=\"left\">Temperatura de revenido<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c (MPa&radic;m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c promedio<\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.05, 20.69<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.58, 20.78<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">149 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.80, 20.90<\/td><td class=\"has-text-align-left\" data-align=\"left\">20.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">63.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.08, 22.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.58, 21.46<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.40, 21.52<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">61.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.31, 22.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.41, 21.96<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">159 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.74, 22.09<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.84, 28.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">36.77, 36.58<\/td><td class=\"has-text-align-left\" data-align=\"left\">36.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">167 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">45.35, 40.08, 41.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">42.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">167 mm red., transversal<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.07, 30.62<\/td><td class=\"has-text-align-left\" data-align=\"left\">30.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">38.63, 38.83<\/td><td class=\"has-text-align-left\" data-align=\"left\">38.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">167 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">371 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">44.18, 46.32<\/td><td class=\"has-text-align-left\" data-align=\"left\">45.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.85, 25.48<\/td><td class=\"has-text-align-left\" data-align=\"left\">25.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">54.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.71, 29.87<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">167 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.12, 32.62<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">58.5<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, Tabla IV, Resultados de las pruebas de tenacidad a la fractura de AISI A2 y D2 de materiales para herramientas para moldes y troqueles.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>A2 se austeniz\u00f3 en sal a 954 &#176;C durante 25 minutos y se enfri\u00f3 al aire, D2 en sal a 1010 &#176;C durante 25 minutos y se enfri\u00f3 al aire. La fila del 88 por ciento revenida a 204 &#176;C marcada como transversal es una sola probeta cortada transversalmente a la barra redonda de 167 mm en lugar de a lo largo, y se lista por separado porque es la \u00fanica lectura transversal de la tabla.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Tenacidad a la fractura de los grados de trabajo en caliente y resistentes al choque (H13 y S7)<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">K1c por reducci\u00f3n de forja, tama\u00f1o de secci\u00f3n, temperatura de revenido y dureza<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Grado<\/th><th class=\"has-text-align-left\" data-align=\"left\">Reducci\u00f3n de forja<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tama\u00f1o de secci\u00f3n<\/th><th class=\"has-text-align-left\" data-align=\"left\">Temperatura de revenido<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c (MPa&radic;m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">K1c promedio<\/th><th class=\"has-text-align-left\" data-align=\"left\">HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.76, 29.89, 29.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">29.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.19, 27.92, 28.18<\/td><td class=\"has-text-align-left\" data-align=\"left\">28.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.63, 26.98, 27.54<\/td><td class=\"has-text-align-left\" data-align=\"left\">27.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">593 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">41.25, 37.50, 38.71<\/td><td class=\"has-text-align-left\" data-align=\"left\">39.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">48.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">593 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.42, 32.74, 31.98<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">47.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">593 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.90, 38.24<\/td><td class=\"has-text-align-left\" data-align=\"left\">37.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">47.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">621 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">87.84, 88.85, 87.74<\/td><td class=\"has-text-align-left\" data-align=\"left\">88.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">621 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">55.02, 80.62, 77.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">71.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H13<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">621 &#176;C, 2h + 2h<\/td><td class=\"has-text-align-left\" data-align=\"left\">59.96, 60.61<\/td><td class=\"has-text-align-left\" data-align=\"left\">60.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.67, 34.41<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">57.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.02, 35.97<\/td><td class=\"has-text-align-left\" data-align=\"left\">35.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">204 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.99, 33.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">33.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">56.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">38.90, 38.41<\/td><td class=\"has-text-align-left\" data-align=\"left\">38.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">53.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">39.48, 39.27<\/td><td class=\"has-text-align-left\" data-align=\"left\">39.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">52.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">496 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.28, 35.13<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">51.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">99%<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.48, 40.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">51.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">95%<\/td><td class=\"has-text-align-left\" data-align=\"left\">89 mm cuadrados<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">40.39, 42.93<\/td><td class=\"has-text-align-left\" data-align=\"left\">41.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">51.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S7<\/td><td class=\"has-text-align-left\" data-align=\"left\">88%<\/td><td class=\"has-text-align-left\" data-align=\"left\">154 mm red.<\/td><td class=\"has-text-align-left\" data-align=\"left\">538 &#176;C, 1h<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.21, 33.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">32.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">50.5<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, Tabla V, Resultados de las pruebas de tenacidad a la fractura de AISI H13 y S7 de materiales para herramientas para moldes y troqueles.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>El H13 se austeniz\u00f3 en sal a 1024 &#176;C durante 25 minutos y se enfri\u00f3 al aire; el S7, en sal a 941 &#176;C durante 25 minutos y se enfri\u00f3 al aire. Las filas del H13 se revenieron dos veces a cada temperatura, dos horas cada vez, que es la pr\u00e1ctica que indican sus fichas t\u00e9cnicas debido a su pico de endurecimiento secundario.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Lo que muestran los ocho grados en comparaci\u00f3n directa<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A la dureza de trabajo normal, los grados se separan en los tres grupos con los que el sector de los \u00fatiles ya trabaja, y la tabla pone cifras a esa separaci\u00f3n. El L6, de temple en aceite, es el m\u00e1s tenaz de los ocho, con valores desde 19,7 MPa ra\u00edz metro a 60 HRC hasta 29,7 a 53,5 HRC. El O2 queda por debajo, con 17,9 a 20,3 en la misma banda de dureza. Le siguen los grados al cromo resistentes al desgaste: el D3 mide 32,8 a 33,7 y el D2 de 25,2 a 45,2 seg\u00fan la secci\u00f3n y el revenido, frente al A2, que mantiene una banda estrecha de 20,9 a 22,3 en todo el intervalo. Los grados para trabajo en caliente y de choque encabezan el conjunto: el S7 alcanza 34,5 a 57 HRC y el H13 va de 27,4 a 88,0 a medida que se reviene desde 53,5 hasta 40,0 HRC.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Dos lecturas de las tablas merecen se\u00f1alarse porque van en contra de la regla general habitual. El D2 midi\u00f3 una tenacidad a la fractura mayor de la que el sector suele atribuirle, en la misma regi\u00f3n que el H13, y su fila del 88 por ciento a 204 &#176;C alcanz\u00f3 42,1 MPa ra\u00edz metro. La otra es la diferencia entre las direcciones longitudinal y transversal en esa misma barra de D2: 42,1 frente a 25,0. Una lectura transversal dice m\u00e1s sobre el molde acabado que una longitudinal, porque un \u00fatil suele fallar en direcci\u00f3n transversal a la direcci\u00f3n de trabajo de la barra, por lo que una especificaci\u00f3n redactada solo sobre la tenacidad longitudinal puede favorecer indebidamente a un grado.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Leer la columna de dureza frente a la tenacidad tambi\u00e9n muestra por qu\u00e9 revenir por debajo de la dureza de trabajo normal no es una forma de comprar seguridad. En las filas del L6, O2, A2 y A6, la tenacidad media aumenta a medida que sube la temperatura de revenido y baja la dureza, y el aumento es constante en lugar de abrupto. Forzar un grado a una dureza menor para ganar tenacidad tambi\u00e9n cuesta resistencia al desgaste, y la tenacidad a\u00f1adida es menor que el salto que dar\u00eda un cambio de grado.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Las cifras son valores experimentales publicados y constituyen \u00fanicamente un resumen de referencia. La tenacidad a la fractura es sensible a la orientaci\u00f3n de la probeta, el tama\u00f1o de la secci\u00f3n y el tratamiento t\u00e9rmico, por lo que las tablas deben tratarse como una comparaci\u00f3n entre grados y no como un valor de dise\u00f1o para una pieza concreta. Confirme con el certificado de ensayo del material o p\u00f3ngase en contacto con Aobo Steel.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Datos de referencia relacionados<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">El aspecto de impacto del mismo tema, medido en probetas Izod sin entalla y Charpy con entalla en V del mismo programa, est\u00e1 en nuestra <a href=\"https:\/\/aobosteel.com\/es\/tool-steel-impact-toughness-chart\/\">Tabla de tenacidad al impacto del acero para herramientas<\/a>. Para la selecci\u00f3n de moldes que convierte esas cifras de tenacidad en una elecci\u00f3n de grado, consulte las p\u00e1ginas de <a href=\"https:\/\/aobosteel.com\/es\/d2-tool-steel\/\">acero para herramientas D2<\/a>, <a href=\"https:\/\/aobosteel.com\/es\/h13-tool-steel\/\">Acero para herramientas H13<\/a>, <a href=\"https:\/\/aobosteel.com\/es\/a2-tool-steel\/\">acero para herramientas A2<\/a> y <a href=\"https:\/\/aobosteel.com\/es\/s7-tool-steel\/\">Acero para herramientas S7<\/a>, y las gu\u00edas sobre <a href=\"https:\/\/aobosteel.com\/es\/tool-steels-for-chipping-resistance\/\">aceros para herramientas resistentes al astillado<\/a> y <a href=\"https:\/\/aobosteel.com\/es\/tool-steels-for-cracking-resistance\/\">aceros para herramientas para resistencia al agrietamiento<\/a>.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Gr\u00e1fico de tenacidad a la fractura del acero para herramientas, PDF imprimible<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">Las cuatro tablas de K1c anteriores, desde L6 y O2 hasta D3, A6, A2, D2, H13 y S7, en un solo PDF con nuestros datos de contacto.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fracture-Toughness-Chart.pdf\">Descargar PDF, 533 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">Fuente: Tool Materials for Molds and Dies, Application and Performance (G. Krauss y H. Nordberg, eds.).<\/p>","protected":false},"excerpt":{"rendered":"<p>Tool Steel Fracture Toughness Chart (K1c) Fracture toughness in MPa root metre for eight common tool steel grades, measured on bend bars taken from three forging reductions and tempered at three temperatures, with the hardness each specimen was tested at. A reference summary of published practice and not an Aobo Steel specification. How the values [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20442","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Tool Steel Fracture Toughness Chart (K1c) | Aobo Steel<\/title>\n<meta name=\"description\" content=\"Fracture toughness (K1c) of L6, O2, D3, A6, A2, D2, H13 and S7 tool steels by forging reduction, section size, tempering temperature and hardness.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/es\/tool-steel-fracture-toughness-chart\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Tool Steel Fracture Toughness Chart (K1c)\" \/>\n<meta property=\"og:description\" content=\"Fracture toughness (K1c) of L6, O2, D3, A6, A2, D2, H13 and S7 tool steels by forging reduction, section size, tempering temperature and hardness.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/es\/tool-steel-fracture-toughness-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:40:35+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"8 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Tool Steel Fracture Toughness Chart (K1c)\",\"datePublished\":\"2026-10-01T01:11:55+00:00\",\"dateModified\":\"2026-10-15T16:40:35+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\"},\"wordCount\":1538,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"es\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\",\"name\":\"Tool Steel Fracture Toughness Chart (K1c) | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-01T01:11:55+00:00\",\"dateModified\":\"2026-10-15T16:40:35+00:00\",\"description\":\"Fracture toughness (K1c) of L6, O2, D3, A6, A2, D2, H13 and S7 tool steels by forging reduction, section size, tempering temperature and hardness.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fracture-toughness-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Tool Steel Fracture Toughness Chart (K1c)\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/es\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tabla de tenacidad a la fractura del acero de herramienta (K1c) | Aobo Steel","description":"Tenacidad a la fractura (K1c) de los aceros L6, O2, D3, A6, A2, D2, H13 y S7 seg\u00fan reducci\u00f3n de forja, tama\u00f1o de secci\u00f3n, temperatura de revenido y dureza.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/es\/tool-steel-fracture-toughness-chart\/","og_locale":"es_ES","og_type":"article","og_title":"Tool Steel Fracture Toughness Chart (K1c)","og_description":"Fracture toughness (K1c) of L6, O2, D3, A6, A2, D2, H13 and S7 tool steels by forging reduction, section size, tempering temperature and hardness.","og_url":"https:\/\/aobosteel.com\/es\/tool-steel-fracture-toughness-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:40:35+00:00","twitter_card":"summary_large_image","twitter_misc":{"Tiempo de lectura":"8 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Tool Steel Fracture Toughness Chart (K1c)","datePublished":"2026-10-01T01:11:55+00:00","dateModified":"2026-10-15T16:40:35+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/"},"wordCount":1538,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"es"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/","url":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/","name":"Tabla de tenacidad a la fractura del acero de herramienta (K1c) | Aobo Steel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-01T01:11:55+00:00","dateModified":"2026-10-15T16:40:35+00:00","description":"Tenacidad a la fractura (K1c) de los aceros L6, O2, D3, A6, A2, D2, H13 y S7 seg\u00fan reducci\u00f3n de forja, tama\u00f1o de secci\u00f3n, temperatura de revenido y dureza.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-fracture-toughness-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Tool Steel Fracture Toughness Chart (K1c)"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tool Steel Fracture Toughness Chart (K1c) Fracture toughness in MPa root metre for eight common tool steel grades, measured on bend bars taken from three forging reductions and tempered at three temperatures, with the hardness each specimen was tested at. A reference summary of published practice and not an Aobo Steel specification. How the values&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tool Steel Fracture Toughness Chart (K1c) Fracture toughness in MPa root metre for eight common tool steel grades, measured on bend bars taken from three forging reductions and tempered at three temperatures, with the hardness each specimen was tested at. A reference summary of published practice and not an Aobo Steel specification. How the values&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20442","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/comments?post=20442"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20442\/revisions"}],"predecessor-version":[{"id":22542,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20442\/revisions\/22542"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/media?parent=20442"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}