{"id":20276,"date":"2026-09-30T00:13:14","date_gmt":"2026-09-29T16:13:14","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20276"},"modified":"2026-10-16T00:20:16","modified_gmt":"2026-10-15T16:20:16","slug":"h13-steel-microstructure-after-quenching","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/es\/h13-steel-microstructure-after-quenching\/","title":{"rendered":"Microestructura del acero H13 despu\u00e9s del temple"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Microestructura del acero H13 despu\u00e9s del temple<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">Perlita, bainita y martensita medidas en bloques de H13 templados en vac\u00edo, gas, sal, aceite y pol\u00edmero, junto a la precipitaci\u00f3n de carburos MC en los l\u00edmites de grano austen\u00edtico para cada temple. Un resumen de referencia de la pr\u00e1ctica publicada y no una especificaci\u00f3n de Aobo Steel.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Lo que decide el temple<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Un dado de H13 se austeniza en la regi\u00f3n de 1010 a 1050 \u00b0C y luego se enfr\u00eda a trav\u00e9s del rango de transformaci\u00f3n. En qu\u00e9 se convierte el acero durante el descenso depende de la velocidad con que atraviesa ese rango, y una secci\u00f3n gruesa no puede disipar calor en su superficie m\u00e1s r\u00e1pido de lo que el n\u00facleo puede ceder calor hacia ella.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">El informe detr\u00e1s de estos datos divide la curva de enfriamiento en dos ventanas. La velocidad entre 1750 y 1550 \u00b0F gobierna cu\u00e1nto carburo MC precipita en los l\u00edmites de grano austen\u00edtico. La velocidad entre 1550 y 750 \u00b0F gobierna la matriz, es decir, cu\u00e1nta perlita, bainita y martensita queda en el dado.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Ambas ventanas se miden a continuaci\u00f3n para los dos tama\u00f1os de bloque extremos del estudio, un cubo de 2 pulgadas y un cubo de 14 pulgadas, templados en diez medios que van desde un vac\u00edo est\u00e1tico hasta una soluci\u00f3n de pol\u00edmero diluida.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Microestructura de la matriz despu\u00e9s del temple<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Las cifras son el porcentaje de cada fase en la superficie del bloque y en su radio medio. B es bainita, M es martensita y P es perlita. Los resultados de gas son para nitr\u00f3geno y helio a 2 atm con una velocidad de gas de 3,400 pies por minuto, que es la condici\u00f3n que el informe us\u00f3 para sus temples en gas. Los ba\u00f1os de sal y las dos soluciones de pol\u00edmero son los medios m\u00e1s r\u00e1pidos de la serie.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Perlita, bainita y martensita por medio de temple<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Medio de temple<\/th><th class=\"has-text-align-left\" data-align=\"left\">Superficie del cubo de 2 pulgadas<\/th><th class=\"has-text-align-left\" data-align=\"left\">Radio medio del cubo de 2 pulgadas<\/th><th class=\"has-text-align-left\" data-align=\"left\">Superficie del cubo de 14 pulgadas<\/th><th class=\"has-text-align-left\" data-align=\"left\">Radio medio del cubo de 14 pulgadas<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Vac\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">28B 72M<\/td><td class=\"has-text-align-left\" data-align=\"left\">28B 72M<\/td><td class=\"has-text-align-left\" data-align=\"left\">13P 72B 15M<\/td><td class=\"has-text-align-left\" data-align=\"left\">14P 72B 14M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitr\u00f3geno<\/td><td class=\"has-text-align-left\" data-align=\"left\">16B 84M<\/td><td class=\"has-text-align-left\" data-align=\"left\">16B 84M<\/td><td class=\"has-text-align-left\" data-align=\"left\">42B 58M<\/td><td class=\"has-text-align-left\" data-align=\"left\">42B 58M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Helio<\/td><td class=\"has-text-align-left\" data-align=\"left\">13B 87M<\/td><td class=\"has-text-align-left\" data-align=\"left\">13B 87M<\/td><td class=\"has-text-align-left\" data-align=\"left\">38B 62M<\/td><td class=\"has-text-align-left\" data-align=\"left\">38B 62M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Aceite de baja velocidad<\/td><td class=\"has-text-align-left\" data-align=\"left\">7B 93M<\/td><td class=\"has-text-align-left\" data-align=\"left\">7B 93M<\/td><td class=\"has-text-align-left\" data-align=\"left\">26B 74M<\/td><td class=\"has-text-align-left\" data-align=\"left\">30B 70M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Al\u00famina fluidizada<\/td><td class=\"has-text-align-left\" data-align=\"left\">5B 95M<\/td><td class=\"has-text-align-left\" data-align=\"left\">5B 95M<\/td><td class=\"has-text-align-left\" data-align=\"left\">23B 77M<\/td><td class=\"has-text-align-left\" data-align=\"left\">29B 71M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Aceite de alta velocidad<\/td><td class=\"has-text-align-left\" data-align=\"left\">2B 98M<\/td><td class=\"has-text-align-left\" data-align=\"left\">2B 98M<\/td><td class=\"has-text-align-left\" data-align=\"left\">15B 85M<\/td><td class=\"has-text-align-left\" data-align=\"left\">27B 73M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Soluci\u00f3n de UCON A al 30%<\/td><td class=\"has-text-align-left\" data-align=\"left\">100M<\/td><td class=\"has-text-align-left\" data-align=\"left\">1B 99M<\/td><td class=\"has-text-align-left\" data-align=\"left\">8B 92M<\/td><td class=\"has-text-align-left\" data-align=\"left\">26B 74M<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Soluci\u00f3n de UCON A al 10%<\/td><td class=\"has-text-align-left\" data-align=\"left\">100M<\/td><td class=\"has-text-align-left\" data-align=\"left\">100M<\/td><td class=\"has-text-align-left\" data-align=\"left\">100M<\/td><td class=\"has-text-align-left\" data-align=\"left\">25B 75M<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, microestructuras de la matriz producidas en funci\u00f3n del medio de temple para los dos tama\u00f1os extremos de bloque de acero H13, Tabla V-16 del informe.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>B es bainita, M es martensita y P es perlita, y las cantidades dentro de cada celda son porcentajes. El informe indica que la superficie y el radio medio del bloque de 2 pulgadas son esencialmente id\u00e9nticos. Las cifras de gas corresponden a nitr\u00f3geno y helio a 2 atm con una velocidad de gas de 3.400 pies por minuto. Solo es una tabla de referencia, no es una recomendaci\u00f3n de Aobo Steel.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Precipitaci\u00f3n de carburos en los l\u00edmites de grano de austenita<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Los carburos MC se forman en los l\u00edmites de grano de austenita mientras el bloque permanece entre 1750 y 1550 \u00b0F, y un temple lento lo mantiene dentro de esa ventana durante m\u00e1s tiempo. El informe da la cantidad como una cifra en una escala de 0 a 100, donde un n\u00famero m\u00e1s alto significa m\u00e1s precipitaci\u00f3n en los l\u00edmites. Los carburos en los l\u00edmites de grano son el rasgo detr\u00e1s de la p\u00e9rdida de ductilidad y tenacidad al impacto que sigue a un temple lento, por lo que esta tabla se lee al rev\u00e9s que la anterior.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Precipitaci\u00f3n de MC en los l\u00edmites de grano seg\u00fan el medio de temple<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Medio de temple<\/th><th class=\"has-text-align-left\" data-align=\"left\">Superficie del cubo de 2 pulgadas<\/th><th class=\"has-text-align-left\" data-align=\"left\">Radio medio del cubo de 2 pulgadas<\/th><th class=\"has-text-align-left\" data-align=\"left\">Superficie del cubo de 14 pulgadas<\/th><th class=\"has-text-align-left\" data-align=\"left\">Radio medio del cubo de 14 pulgadas<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Vac\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">91<\/td><td class=\"has-text-align-left\" data-align=\"left\">91<\/td><td class=\"has-text-align-left\" data-align=\"left\">98<\/td><td class=\"has-text-align-left\" data-align=\"left\">98<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitr\u00f3geno<\/td><td class=\"has-text-align-left\" data-align=\"left\">74<\/td><td class=\"has-text-align-left\" data-align=\"left\">74<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><td class=\"has-text-align-left\" data-align=\"left\">96<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Helio<\/td><td class=\"has-text-align-left\" data-align=\"left\">68<\/td><td class=\"has-text-align-left\" data-align=\"left\">68<\/td><td class=\"has-text-align-left\" data-align=\"left\">92<\/td><td class=\"has-text-align-left\" data-align=\"left\">96<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Aceite de baja velocidad<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">52<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Sal a 750 \u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Al\u00famina fluidizada<\/td><td class=\"has-text-align-left\" data-align=\"left\">44<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">51<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Sal a 575 \u00b0F<\/td><td class=\"has-text-align-left\" data-align=\"left\">28<\/td><td class=\"has-text-align-left\" data-align=\"left\">41<\/td><td class=\"has-text-align-left\" data-align=\"left\">32<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Aceite de alta velocidad<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">93<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Soluci\u00f3n de UCON A al 30%<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">27<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">92<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Soluci\u00f3n de UCON A al 10%<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">0<\/td><td class=\"has-text-align-left\" data-align=\"left\">92<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, precipitaci\u00f3n de MC en los l\u00edmites de grano en funci\u00f3n del medio de temple para los dos tama\u00f1os extremos de bloque de acero H13, Tabla IV-15 del informe.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Las cifras est\u00e1n en la escala de 0 a 100 que usa el informe, donde un n\u00famero m\u00e1s alto significa m\u00e1s precipitaci\u00f3n de carburos MC en los l\u00edmites de grano de austenita. Las dos entradas de ba\u00f1o de sal aparecen solo en esta tabla, y el ba\u00f1o a 575 \u00b0F es el m\u00e1s r\u00e1pido de los dos. Solo es una tabla de referencia, no es una recomendaci\u00f3n de Aobo Steel.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Lectura conjunta de las dos tablas<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">En el cubo de 2 pulgadas, la superficie y el radio medio dan la misma lectura, porque una secci\u00f3n tan peque\u00f1a no puede mantener una diferencia de temperatura a trav\u00e9s de s\u00ed misma el tiempo suficiente para que importe. El temple al vac\u00edo deja la mayor cantidad de bainita, con 28% frente a 72% de martensita, y la cantidad disminuye con cada aumento en la velocidad de enfriamiento, hasta 2% en aceite de alta velocidad. Ambas soluciones polim\u00e9ricas llevan ese bloque a totalmente martens\u00edtico.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">En el cubo de 14 pulgadas los mismos medios se comportan de manera muy diferente. El radio medio queda entre 25% y 72% de bainita sea cual sea el temple, porque el calor tiene que viajar hacia afuera a trav\u00e9s del propio acero y la superficie deja de controlar el n\u00facleo. En la superficie solo la soluci\u00f3n UCON A al 10% alcanza totalmente martens\u00edtico, y el temple al vac\u00edo es lo suficientemente lento como para dejar perlita en la estructura en ambas posiciones.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">La precipitaci\u00f3n de MC va en sentido contrario. El temple al vac\u00edo punt\u00faa de 91 a 98 en la escala, y las dos soluciones polim\u00e9ricas punt\u00faan 0 en la superficie de ambos bloques. En el radio medio del cubo de 14 pulgadas todo temple queda entre 92 y 98, que es el mismo mensaje que la tabla de matriz le\u00edda en sentido opuesto, que el centro de un bloque grueso de H13 lo define el acero y casi nada el medio que lo rodea.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Microestructura del acero H13 despu\u00e9s del temple, PDF imprimible<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">Ambas tablas de esta p\u00e1gina, la microestructura de la matriz y la precipitaci\u00f3n de MC en los l\u00edmites de grano para los dos tama\u00f1os extremos de bloque de H13, en un PDF con nuestros datos de contacto.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-H13-Steel-Microstructure-After-Quenching.pdf\">Descargar PDF, 391 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">Datos de referencia relacionados<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">El grado al que pertenecen estos datos se describe en la <a href=\"https:\/\/aobosteel.com\/es\/h13-tool-steel\/\">p\u00e1gina del acero para herramientas H13<\/a>, y las velocidades de enfriamiento detr\u00e1s de estas microestructuras est\u00e1n en la <a href=\"https:\/\/aobosteel.com\/es\/h13-quenching-cooling-rates\/\">p\u00e1gina de velocidades de enfriamiento del temple de H13<\/a>. El resto del ciclo alrededor del temple est\u00e1 en la <a href=\"https:\/\/aobosteel.com\/es\/h13-steel-heat-treatment\/\">Gu\u00eda de tratamiento t\u00e9rmico H13<\/a>, con la dureza de servicio que debe alcanzar en la <a href=\"https:\/\/aobosteel.com\/es\/h13-steel-hardness\/\">Tabla de dureza del H13<\/a>. C\u00f3mo se ve un temple que sale mal se cubre en la <a href=\"https:\/\/aobosteel.com\/es\/quench-cracking-tool-steel\/\">p\u00e1gina de agrietamiento durante el temple<\/a>, los grados que se endurecen al aire quieto se separan en la <a href=\"https:\/\/aobosteel.com\/es\/air-hardening-tool-steel\/\">p\u00e1gina de acero para herramientas de templado al aire<\/a>, y el aspecto de este mismo grado para fundici\u00f3n a presi\u00f3n est\u00e1 en la <a href=\"https:\/\/aobosteel.com\/es\/tool-steel-for-die-casting-dies-inserts\/\">p\u00e1gina de troqueles e insertos para fundici\u00f3n a presi\u00f3n<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fuente: Improved Life of Die Casting Dies of H13 Steel by Attaining Improved Mechanical Properties and Distortion Control During Heat Treatment (J. F. Wallace and D. Schwam, US Department of Energy final report DOE\/ID\/13320-3, October 1998).<\/p>","protected":false},"excerpt":{"rendered":"<p>H13 Steel Microstructure After Quenching Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, set beside the MC carbide precipitation at the austenite grain boundaries for each quench. A reference summary of published practice and not an Aobo Steel specification. What the quench decides An H13 die is [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20276","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>H13 Steel Microstructure After Quenching<\/title>\n<meta name=\"description\" content=\"Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, with the MC carbide precipitation at the austenite grain boundaries.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/es\/h13-steel-microstructure-after-quenching\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"H13 Steel Microstructure After Quenching\" \/>\n<meta property=\"og:description\" content=\"Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, with the MC carbide precipitation at the austenite grain boundaries.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/es\/h13-steel-microstructure-after-quenching\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:20:16+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"5 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"H13 Steel Microstructure After Quenching\",\"datePublished\":\"2026-09-29T16:13:14+00:00\",\"dateModified\":\"2026-10-15T16:20:16+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\"},\"wordCount\":1058,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"es\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\",\"name\":\"H13 Steel Microstructure After Quenching\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-29T16:13:14+00:00\",\"dateModified\":\"2026-10-15T16:20:16+00:00\",\"description\":\"Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, with the MC carbide precipitation at the austenite grain boundaries.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/h13-steel-microstructure-after-quenching\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"H13 Steel Microstructure After Quenching\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/es\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Microestructura del acero H13 despu\u00e9s del temple","description":"Perlita, bainita y martensita medidas en bloques H13 templados en vac\u00edo, gas, sal, aceite y pol\u00edmero, con la precipitaci\u00f3n de carburos MC en los l\u00edmites de grano austen\u00edtico.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/es\/h13-steel-microstructure-after-quenching\/","og_locale":"es_ES","og_type":"article","og_title":"H13 Steel Microstructure After Quenching","og_description":"Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, with the MC carbide precipitation at the austenite grain boundaries.","og_url":"https:\/\/aobosteel.com\/es\/h13-steel-microstructure-after-quenching\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:20:16+00:00","twitter_card":"summary_large_image","twitter_misc":{"Tiempo de lectura":"5 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"H13 Steel Microstructure After Quenching","datePublished":"2026-09-29T16:13:14+00:00","dateModified":"2026-10-15T16:20:16+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/"},"wordCount":1058,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"es"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/","url":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/","name":"Microestructura del acero H13 despu\u00e9s del temple","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-29T16:13:14+00:00","dateModified":"2026-10-15T16:20:16+00:00","description":"Perlita, bainita y martensita medidas en bloques H13 templados en vac\u00edo, gas, sal, aceite y pol\u00edmero, con la precipitaci\u00f3n de carburos MC en los l\u00edmites de grano austen\u00edtico.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/h13-steel-microstructure-after-quenching\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"H13 Steel Microstructure After Quenching"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"H13 Steel Microstructure After Quenching Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, set beside the MC carbide precipitation at the austenite grain boundaries for each quench. A reference summary of published practice and not an Aobo Steel specification. What the quench decides An H13 die is&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"H13 Steel Microstructure After Quenching Pearlite, bainite and martensite measured in H13 blocks quenched in vacuum, gas, salt, oil and polymer, set beside the MC carbide precipitation at the austenite grain boundaries for each quench. A reference summary of published practice and not an Aobo Steel specification. What the quench decides An H13 die is&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20276","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/comments?post=20276"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20276\/revisions"}],"predecessor-version":[{"id":22507,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/20276\/revisions\/22507"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/media?parent=20276"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}