{"id":19910,"date":"2026-09-27T04:11:55","date_gmt":"2026-09-26T20:11:55","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=19910"},"modified":"2026-10-16T00:08:43","modified_gmt":"2026-10-15T16:08:43","slug":"a6-tool-steel-heat-treatment","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/es\/a6-tool-steel-heat-treatment\/","title":{"rendered":"Tratamiento t\u00e9rmico del acero para herramientas A6"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Tratamiento t\u00e9rmico del acero para herramientas A6<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">El A6 se ubica en el grupo de trabajo en fr\u00edo templado al aire, y las cifras a continuaci\u00f3n son lo que un taller necesita para llevar el grado a trav\u00e9s de un horno. La temperatura de temple, el medio de enfriamiento y la dureza que deja cada temperatura de revenido se presentan tal como los publica la ficha de origen. Un resumen de referencia de la pr\u00e1ctica publicada y no una especificaci\u00f3n de Aobo Steel.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">A6 en el grupo de trabajo en fr\u00edo templado al aire<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">El A6 contiene aproximadamente 2% de manganeso sobre una base de 0.70% de carbono, con cromo al 1.00% y molibdeno al 1.30%. El manganeso es lo que aporta la templabilidad del grado, y es la raz\u00f3n por la que el A6 se templa al aire mientras su cromo se mantiene por debajo del 1.5%. Eso coloca al grado en el grupo de trabajo en fr\u00edo templado al aire, que es el grupo que se elige cuando una herramienta debe mantener su tama\u00f1o a trav\u00e9s del tratamiento t\u00e9rmico y no se desea un enfriamiento l\u00edquido. El A2 se ubica en el mismo grupo y alcanza el temple al aire desde un nivel de cromo mucho m\u00e1s alto.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">La ficha es informaci\u00f3n de referencia para el taller m\u00e1s que una especificaci\u00f3n. Da al grado un paso de precalentamiento, una temperatura de temple y un medio de enfriamiento, luego una tabla de revenido en pasos de 100 \u00b0F con una sola cifra de dureza en cada fila. La tabla termina a 600 \u00b0F (315 \u00b0C) y no hay bandas de tolerancia en ninguna parte de la ficha, por lo que vale la pena probar una primera herramienta cortada de una nueva colada de acero como ensayo antes de que el ciclo pase a un troquel de producci\u00f3n.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">En condici\u00f3n recocida el grado llega a 217 a 248 HB, la cifra que imprime para el A6 la tabla de temperaturas de recocido y normalizado de este sitio, donde el grado tambi\u00e9n figura como uno que no se normaliza. La misma tabla da el rango de recocido como 730 a 745 \u00b0C (1350 a 1375 \u00b0F) con una velocidad m\u00e1xima de enfriamiento de 14 \u00b0C\/h (25 \u00b0F\/h).<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Composici\u00f3n qu\u00edmica del A6<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">Elementos que la ficha de referencia enumera, porcentaje<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Elemento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Porcentaje<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Carbono<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Manganese<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Silicon<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Cromo<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Molibdeno<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.30<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, informaci\u00f3n de referencia de tratamiento t\u00e9rmico para A6, p\u00e1gina impresa 182.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>La ficha imprime una cifra para cada elemento en lugar de un rango de especificaci\u00f3n. El vanadio, el tungsteno, el cobalto y el azufre aparecen en la ficha sin cifra alguna y se omiten de la tabla en lugar de mostrarse como cero.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">El manganeso al 2.00% es la cifra que distingue al A6, y es alta para un acero para herramientas. Con cromo al 1.00% y molibdeno al 1.30%, el manganeso es lo que da al grado suficiente templabilidad para salir duro de un temple al aire, que es por lo que la tabla de temple de esta p\u00e1gina imprime aire como medio de enfriamiento. El carbono al 0.70% fija la dureza desde la que parte la tabla de revenido, y el silicio al 0.30% proviene de la pr\u00e1ctica de fusi\u00f3n. La tabla de composici\u00f3n de este sitio lista el A6 como UNS T30106 con carbono de 0.65 a 0.75%, manganeso de 1.80 a 2.50%, cromo de 0.90 a 1.20% y molibdeno de 0.90 a 1.40%, por lo que cada cifra de esta ficha se ubica dentro del rango que la norma da al grado. La ficha lista vanadio, tungsteno, cobalto y azufre sin cifra alguna, por lo que esas filas se omiten de la tabla en lugar de imprimirse como cero. Los datos de composici\u00f3n de la tabla son solo para referencia general, los valores reales var\u00edan seg\u00fan norma, acer\u00eda y n\u00famero de colada, as\u00ed que confirme las cifras contra el certificado de ensayo del material de la colada o consulte a Aobo Steel.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Temple del A6<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">Precalentamiento, temperatura de temple y enfriamiento<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Paso<\/th><th class=\"has-text-align-left\" data-align=\"left\">A6<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Precalentamiento<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200 \u00b0F (650 \u00b0C)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Templar<\/td><td class=\"has-text-align-left\" data-align=\"left\">1575 \u00b0F (855 \u00b0C)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Medio de temple<\/td><td class=\"has-text-align-left\" data-align=\"left\">Temple al aire<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, informaci\u00f3n de referencia de tratamiento t\u00e9rmico para A6, p\u00e1gina impresa 182.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>La ficha no asocia ninguna condici\u00f3n de tama\u00f1o al precalentamiento, por lo que el paso no est\u00e1 marcado como uno que solo necesiten las secciones m\u00e1s grandes. Imprime una temperatura de temple y un medio de enfriamiento para el grado, sin alternativa en aceite o sales junto al enfriamiento al aire.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">El precalentamiento de 1200 \u00b0F (650 \u00b0C) es la misma cifra que imprime para el A6 la tabla de temple y revenido de este sitio, y la ficha no le atribuye ninguna condici\u00f3n de tama\u00f1o, por lo que el paso aplica a toda carga y no solo a las pesadas. El temple se realiza a 1575 \u00b0F (855 \u00b0C) al aire. La misma tabla da al grado una banda de temple de 1525 a 1600 \u00b0F (830 a 870 \u00b0C) con 20 a 45 minutos a temperatura, por lo que la cifra \u00fanica de esta ficha se ubica dentro de esa banda y el temple al aire que imprime es el enfriamiento que lista la tabla. La ficha no imprime ning\u00fan medio de enfriamiento alternativo, por lo que la velocidad de enfriamiento queda sujeta al suministro de aire del taller y a la secci\u00f3n que entra al horno.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Respuesta al revenido del A6<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">Dureza que deja cada temperatura de revenido<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Revenido, \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">A6, HRC<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Reci\u00e9n templado<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sin revenido<\/td><td class=\"has-text-align-left\" data-align=\"left\">67<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">64<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">400<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">61<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">500<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">59<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fuente, informaci\u00f3n de referencia de tratamiento t\u00e9rmico para A6, p\u00e1gina impresa 182.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>La ficha escalona las temperaturas de revenido en pasos de 100 \u00b0F desde 300 \u00b0F hasta 600 \u00b0F e imprime una cifra Rockwell C para cada una. La primera fila es la dureza tal como se templa, antes de cualquier revenido, y la ficha no contiene ninguna fila por encima de 600 \u00b0F.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">El temple deja el grado a 67 HRC tal como se templa y el primer revenido a 300 \u00b0F (150 \u00b0C) lo baja a 64 HRC. A partir de ah\u00ed la l\u00ednea se mueve con cada paso, 61 HRC a 400 \u00b0F (205 \u00b0C), 59 HRC a 500 \u00b0F (260 \u00b0C) y 55 HRC a 600 \u00b0F (315 \u00b0C). La ficha termina a 600 \u00b0F, mientras que la tabla de temple y revenido de este sitio lista la banda de revenido del grado como 300 a 800 \u00b0F (150 a 425 \u00b0C), por lo que la parte superior de esa banda no est\u00e1 cubierta por esta ficha. El revenido del A6 es una elecci\u00f3n entre la dureza de las filas superiores y la tenacidad que aporta un revenido m\u00e1s alto, y una herramienta que debe resistir el desportillamiento en servicio normalmente se reviene hacia la parte superior de la banda en lugar de la inferior.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Tratamiento t\u00e9rmico del acero para herramientas A6, PDF imprimible<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">La composici\u00f3n qu\u00edmica, el ciclo de temple y la respuesta al revenido del A6 de esta p\u00e1gina en un solo PDF, con nuestros datos de contacto.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-A6-Tool-Steel-Heat-Treatment.pdf\">Descargar PDF, 369 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">Datos de referencia relacionados<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">El grado m\u00e1s cercano en el mismo grupo es el A2 y su ciclo est\u00e1 en la <a href=\"https:\/\/aobosteel.com\/es\/a2-tool-steel-heat-treatment-guide\/\">p\u00e1gina de tratamiento t\u00e9rmico del acero para herramientas A2<\/a>. Lo que el temple al aire hace por el movimiento dimensional y d\u00f3nde se pone a trabajar el grado se exponen en la <a href=\"https:\/\/aobosteel.com\/es\/air-hardening-tool-steel\/\">p\u00e1gina de acero para herramientas templado al aire<\/a>. Las bandas de temple y revenido en los grupos de aceros para herramientas est\u00e1n en la <a href=\"https:\/\/aobosteel.com\/es\/tool-steel-hardening-tempering-chart\/\">tabla de temple y revenido del acero para herramientas<\/a>, el rango de composici\u00f3n del A6 est\u00e1 en la <a href=\"https:\/\/aobosteel.com\/es\/tool-steel-composition-chart\/\">Tabla de composici\u00f3n del acero para herramientas<\/a>, su dureza recocida y velocidad de enfriamiento est\u00e1n en la <a href=\"https:\/\/aobosteel.com\/es\/tool-steel-annealing-normalizing-temperature-chart\/\">tabla de temperaturas de recocido y normalizado para acero para herramientas<\/a>, la maquinabilidad de la serie A est\u00e1 en la <a href=\"https:\/\/aobosteel.com\/es\/tool-steel-machinability-rating-chart\/\">Tabla de clasificaci\u00f3n de maquinabilidad del acero para herramientas<\/a>, y el rango de dureza de trabajo est\u00e1 en la <a href=\"https:\/\/aobosteel.com\/es\/tool-steel-properties-chart\/\">tabla de propiedades del acero para herramientas<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Datos de referencia recopilados de Heat Treatment, Selection, and Application of Tool Steels (William E. Bryson, segunda edici\u00f3n, Hanser). La composici\u00f3n qu\u00edmica, el ciclo de temple y la respuesta al revenido del A6 provienen de la informaci\u00f3n de referencia de tratamiento t\u00e9rmico de la p\u00e1gina impresa 182.<\/p>","protected":false},"excerpt":{"rendered":"<p>A6 Tool Steel Heat Treatment A6 sits in the air-hardening cold work group, and the figures below are what a shop needs to put the grade through a furnace. The hardening temperature, the quench medium and the hardness left by each tempering temperature are set out as the source card publishes them. A reference summary [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-19910","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>A6 Tool Steel Heat Treatment Chart and Tempering Data<\/title>\n<meta name=\"description\" content=\"The hardening temperature, air quench and tempering response of A6 tool steel, with its chemistry and the hardness left at each tempering temperature.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/es\/a6-tool-steel-heat-treatment\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"A6 Tool Steel Heat Treatment\" \/>\n<meta property=\"og:description\" content=\"The hardening temperature, air quench and tempering response of A6 tool steel, with its chemistry and the hardness left at each tempering temperature.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/es\/a6-tool-steel-heat-treatment\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:08:43+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"6 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a6-tool-steel-heat-treatment\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a6-tool-steel-heat-treatment\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"A6 Tool Steel Heat Treatment\",\"datePublished\":\"2026-09-26T20:11:55+00:00\",\"dateModified\":\"2026-10-15T16:08:43+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a6-tool-steel-heat-treatment\\\/\"},\"wordCount\":1115,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"es\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a6-tool-steel-heat-treatment\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/a6-tool-steel-heat-treatment\\\/\",\"name\":\"A6 Tool Steel Heat Treatment Chart and Tempering Data\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-26T20:11:55+00:00\",\"dateModified\":\"2026-10-15T16:08:43+00:00\",\"description\":\"The hardening temperature, air quench and tempering response of A6 tool steel, with its chemistry and the hardness left at each tempering temperature.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a6-tool-steel-heat-treatment\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/a6-tool-steel-heat-treatment\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/a6-tool-steel-heat-treatment\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"A6 Tool Steel Heat Treatment\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/es\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tabla de tratamiento t\u00e9rmico y datos de revenido del acero para herramientas A6","description":"La temperatura de austenizaci\u00f3n, temple en aire y respuesta al revenido del acero para herramientas A6, con su composici\u00f3n qu\u00edmica y la dureza resultante a cada temperatura de revenido.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/es\/a6-tool-steel-heat-treatment\/","og_locale":"es_ES","og_type":"article","og_title":"A6 Tool Steel Heat Treatment","og_description":"The hardening temperature, air quench and tempering response of A6 tool steel, with its chemistry and the hardness left at each tempering temperature.","og_url":"https:\/\/aobosteel.com\/es\/a6-tool-steel-heat-treatment\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:08:43+00:00","twitter_card":"summary_large_image","twitter_misc":{"Tiempo de lectura":"6 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/a6-tool-steel-heat-treatment\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/a6-tool-steel-heat-treatment\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"A6 Tool Steel Heat Treatment","datePublished":"2026-09-26T20:11:55+00:00","dateModified":"2026-10-15T16:08:43+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/a6-tool-steel-heat-treatment\/"},"wordCount":1115,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"es"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/a6-tool-steel-heat-treatment\/","url":"https:\/\/aobosteel.com\/a6-tool-steel-heat-treatment\/","name":"Tabla de tratamiento t\u00e9rmico y datos de revenido del acero para herramientas A6","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-26T20:11:55+00:00","dateModified":"2026-10-15T16:08:43+00:00","description":"La temperatura de austenizaci\u00f3n, temple en aire y respuesta al revenido del acero para herramientas A6, con su composici\u00f3n qu\u00edmica y la dureza resultante a cada temperatura de revenido.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/a6-tool-steel-heat-treatment\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/a6-tool-steel-heat-treatment\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/a6-tool-steel-heat-treatment\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"A6 Tool Steel Heat Treatment"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"A6 Tool Steel Heat Treatment A6 sits in the air-hardening cold work group, and the figures below are what a shop needs to put the grade through a furnace. The hardening temperature, the quench medium and the hardness left by each tempering temperature are set out as the source card publishes them. A reference summary&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"A6 Tool Steel Heat Treatment A6 sits in the air-hardening cold work group, and the figures below are what a shop needs to put the grade through a furnace. The hardening temperature, the quench medium and the hardness left by each tempering temperature are set out as the source card publishes them. A reference summary&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/19910","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/comments?post=19910"}],"version-history":[{"count":5,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/19910\/revisions"}],"predecessor-version":[{"id":22485,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/19910\/revisions\/22485"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/media?parent=19910"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}