{"id":19422,"date":"2026-09-21T13:28:57","date_gmt":"2026-09-21T05:28:57","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=19422"},"modified":"2026-10-16T10:28:40","modified_gmt":"2026-10-16T02:28:40","slug":"austenitic-stainless-steel-mechanical-properties","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/es\/austenitic-stainless-steel-mechanical-properties\/","title":{"rendered":"Austenitic Stainless Steel Mechanical Properties Chart"},"content":{"rendered":"<h1 id=\"h-mechanical-properties-of-austenitic-stainless-steels\" class=\"wp-block-heading\">Propiedades mec\u00e1nicas de los aceros inoxidables austen\u00edticos<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">Resistencia m\u00ednima a la tracci\u00f3n y al l\u00edmite el\u00e1stico a temperatura ambiente, alargamiento, reducci\u00f3n de \u00e1rea y dureza para los aceros inoxidables austen\u00edticos forjados, indicados para cada forma de producto y condici\u00f3n con la especificaci\u00f3n ASTM que contiene el requisito. Un m\u00ednimo es el l\u00edmite que una colada debe superar, por lo que un certificado generalmente muestra m\u00e1s.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Los valores m\u00ednimos que cada forma de producto y condici\u00f3n debe cumplir, con la especificaci\u00f3n ASTM que contiene el requisito. Tabla 7 de la fuente.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">UNS<\/th><th class=\"has-text-align-left\" data-align=\"left\">Forma<\/th><th class=\"has-text-align-left\" data-align=\"left\">Condici\u00f3n<\/th><th class=\"has-text-align-left\" data-align=\"left\">De tensi\u00f3n<br>MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">De tensi\u00f3n<br>ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">L\u00edmite el\u00e1stico 0,2 %<br>MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">L\u00edmite el\u00e1stico 0,2 %<br>ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">Alarg.<br>%<\/th><th class=\"has-text-align-left\" data-align=\"left\">Red. de<br>\u00e1rea, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza<br>HRB<\/th><th class=\"has-text-align-left\" data-align=\"left\">ASTM<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 301<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 301<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 301<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/4 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">860<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 301<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/2 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1030<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">18<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 301<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">3\/4 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1210<\/td><td class=\"has-text-align-left\" data-align=\"left\">175<\/td><td class=\"has-text-align-left\" data-align=\"left\">930<\/td><td class=\"has-text-align-left\" data-align=\"left\">135<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 301<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Totalmente duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1280<\/td><td class=\"has-text-align-left\" data-align=\"left\">185<\/td><td class=\"has-text-align-left\" data-align=\"left\">965<\/td><td class=\"has-text-align-left\" data-align=\"left\">140<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240, A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Alta resistencia a la tracci\u00f3n, 1\/4 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">860<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Alta resistencia a la tracci\u00f3n, 1\/2 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1030<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Alta resistencia a la tracci\u00f3n, 3\/4 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1205<\/td><td class=\"has-text-align-left\" data-align=\"left\">175<\/td><td class=\"has-text-align-left\" data-align=\"left\">930<\/td><td class=\"has-text-align-left\" data-align=\"left\">135<\/td><td class=\"has-text-align-left\" data-align=\"left\">6<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Totalmente duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1275<\/td><td class=\"has-text-align-left\" data-align=\"left\">185<\/td><td class=\"has-text-align-left\" data-align=\"left\">965<\/td><td class=\"has-text-align-left\" data-align=\"left\">140<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302B<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30215<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302B<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30215<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302B<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30215<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302B<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30215<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302B<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30215<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302B<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30215<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302Cu<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30430<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<sup>(e)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 493<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 302Cu<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30430<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<sup>(e)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">Ligeramente trefilado<\/td><td class=\"has-text-align-left\" data-align=\"left\">585<\/td><td class=\"has-text-align-left\" data-align=\"left\">85<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 493<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 303 y 303Se<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30300, S30323<\/td><td class=\"has-text-align-left\" data-align=\"left\">F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 303 y 303Se<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30300, S30323<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">585\u2013860<\/td><td class=\"has-text-align-left\" data-align=\"left\">85\u2013125<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 303 y 303Se<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30300, S30323<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trabajado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">790\u20131000<\/td><td class=\"has-text-align-left\" data-align=\"left\">115\u2013145<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 581<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<sup>(f)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/8 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/4 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">860<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/2 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1035<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">88 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304B4<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30424<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St grado A<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">27<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 887<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304B4<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30424<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St grado B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 887<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">88 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Alta resistencia a la tracci\u00f3n<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">1690<\/td><td class=\"has-text-align-left\" data-align=\"left\">245<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Cronifer 18-15 LCSi<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30600<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">540<\/td><td class=\"has-text-align-left\" data-align=\"left\">78<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 308<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30800<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 308<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30800<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 308<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30800<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 308<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30800<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 308<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30800<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 308<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30800<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">88 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 309, 309S, 310 y 310S<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30900, S30908, S31000, S31008<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 309, 309S, 310 y 310S<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30900, S30908, S31000, S31008<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 309, 309S, 310 y 310S<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30900, S30908, S31000, S31008<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 309, 309S, 310 y 310S<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30900, S30908, S31000, S31008<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 309, 309S, 310 y 310S<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30900, S30908, S31000, S31008<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 309, 309S, 310 y 310S<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30900, S30908, S31000, S31008<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31040<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31040<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, Perfiles<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31040<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, Perfiles<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31040<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, Perfiles<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31040<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31040<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 314<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 314<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 314<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31400<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 314<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31400<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 314<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31400<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31600<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<sup>(f)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31600<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31600<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31600<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31600<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31600<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">480<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31640<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31640<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, Perfiles<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31640<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, Perfiles<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31640<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, Perfiles<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31640<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316Cb<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31640<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31700<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31700<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31700<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31700<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31700<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31700<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31703<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">585<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">85<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">240<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">55<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">65<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">85 m\u00e1x<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31703<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317LM<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31725<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317LM<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31725<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 321 y 321H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32100, S32109<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 321 y 321H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32100, S32109<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 321 y 321H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32100, S32109<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 321 y 321H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32100, S32109<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 321 y 321H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32100, S32109<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 321 y 321H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32100, S32109<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 347 y 348<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34700, S34800<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\"><\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 347 y 348<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34700, S34800<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(b) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 347 y 348<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34700, S34800<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo(c) y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 347 y 348<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34700, S34800<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">50<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 347 y 348<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34700, S34800<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<sup>(d)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 347 y 348<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34700, S34800<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">18-18-2<\/td><td class=\"has-text-align-left\" data-align=\"left\">S38100<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 384<\/td><td class=\"has-text-align-left\" data-align=\"left\">S38400<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<sup>(e)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 493<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 384<\/td><td class=\"has-text-align-left\" data-align=\"left\">S38400<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<sup>(e)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">Ligeramente trefilado<\/td><td class=\"has-text-align-left\" data-align=\"left\">585<\/td><td class=\"has-text-align-left\" data-align=\"left\">85<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 493<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20Cb-3, 20Mo-4 y 20Mo-6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08020, N08024, N08026<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20Cb-3, 20Mo-4 y 20Mo-6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08020, N08024, N08026<\/td><td class=\"has-text-align-left\" data-align=\"left\">Formas<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20Cb-3, 20Mo-4 y 20Mo-6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08020, N08024, N08026<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido y endurecido por deformaci\u00f3n<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">415<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20Cb-3, 20Mo-4 y 20Mo-6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08020, N08024, N08026<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido y acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620\u2013830<\/td><td class=\"has-text-align-left\" data-align=\"left\">90\u2013120<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 473<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20Cb-3, 20Mo-4 y 20Mo-6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08020, N08024, N08026<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 463<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20Cb-3, 20Mo-4 y 20Mo-6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08020, N08024, N08026<\/td><td class=\"has-text-align-left\" data-align=\"left\">Pi, T<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 464, B 468, B 474, B 729<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Sanicro 28<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08028<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">500<\/td><td class=\"has-text-align-left\" data-align=\"left\">73<\/td><td class=\"has-text-align-left\" data-align=\"left\">215<\/td><td class=\"has-text-align-left\" data-align=\"left\">31<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">70-90<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">B 709<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Sanicro 28<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08028<\/td><td class=\"has-text-align-left\" data-align=\"left\">Tubo sin costura<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">500<\/td><td class=\"has-text-align-left\" data-align=\"left\">73<\/td><td class=\"has-text-align-left\" data-align=\"left\">215<\/td><td class=\"has-text-align-left\" data-align=\"left\">31<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 668<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 330<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08330<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 511<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 330<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08330<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">70-90<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">B 536<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 330<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08330<\/td><td class=\"has-text-align-left\" data-align=\"left\">Pi<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">485<\/td><td class=\"has-text-align-left\" data-align=\"left\">70<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">70-90<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">B 535, B 546<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL-6X<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08366<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 691<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL-6X<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08366<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 688<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL-6X<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08366<\/td><td class=\"has-text-align-left\" data-align=\"left\">Pi, T<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 675, B 676, B 690<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL-6X<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08366<\/td><td class=\"has-text-align-left\" data-align=\"left\">T soldado<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trabajado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 676<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">JS-700<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08700<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 672<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">JS-700<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08700<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">75-90<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">B 599<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 332<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08800<\/td><td class=\"has-text-align-left\" data-align=\"left\">Pi, T<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 163, B 407, B 514, B 515<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 332<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08800<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sin costura Pi, T<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en caliente<\/td><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">170<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 407<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 332<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08800<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trabajado en caliente<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 408<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 332<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08800<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 408<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 332<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08800<\/td><td class=\"has-text-align-left\" data-align=\"left\">P<\/td><td class=\"has-text-align-left\" data-align=\"left\">Laminado en caliente<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 409<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 332<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08800<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">210<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 409<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 904L<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08904<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">490<\/td><td class=\"has-text-align-left\" data-align=\"left\">71<\/td><td class=\"has-text-align-left\" data-align=\"left\">220<\/td><td class=\"has-text-align-left\" data-align=\"left\">31<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 649<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 904L<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08904<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Acabado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">620\u2013830<\/td><td class=\"has-text-align-left\" data-align=\"left\">90\u2013120<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 649<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 904L<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08904<\/td><td class=\"has-text-align-left\" data-align=\"left\">Pi, T<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">490<\/td><td class=\"has-text-align-left\" data-align=\"left\">71<\/td><td class=\"has-text-align-left\" data-align=\"left\">220<\/td><td class=\"has-text-align-left\" data-align=\"left\">31<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B 673, B 674, B 677<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 904L<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08904<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">490<\/td><td class=\"has-text-align-left\" data-align=\"left\">71<\/td><td class=\"has-text-align-left\" data-align=\"left\">220<\/td><td class=\"has-text-align-left\" data-align=\"left\">31<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">70-90<sup>(g)<\/sup><\/td><td class=\"has-text-align-left\" data-align=\"left\">B 625<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Fuente: ASM Handbook, Vol 1 (10.\u00aa ed.), &#8220;Wrought Stainless Steels&#8221;, Tabla 7.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Propiedades mec\u00e1nicas del acero inoxidable austen\u00edtico, PDF para imprimir<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Tres p\u00e1ginas A4 con los valores m\u00ednimos de resistencia a la tracci\u00f3n y l\u00edmite el\u00e1stico, alargamiento, reducci\u00f3n de \u00e1rea y dureza de 147 filas de tipo, forma de producto y estado, la especificaci\u00f3n ASTM indicada en cada fila y nuestros datos de contacto. El PDF est\u00e1 en ingl\u00e9s.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Austenitic-Stainless-Mechanical-Properties.pdf\">Descargar PDF, 707 KB<\/a><\/div>\n<\/div>\n<\/div>\n\n\n\n<ul class=\"wp-block-list\">\n<li><sup>(a)<\/sup> B, barra; F, forjados; P, placa; Pi, tuber\u00eda; Sh, chapa; St, fleje; T, tubo; W, alambre.<\/li>\n\n\n\n<li><sup>(b)<\/sup> Hasta 13 mm (0.5 in.) de espesor.<\/li>\n\n\n\n<li><sup>(c)<\/sup> M\u00e1s de 13 mm (0.5 in.) de espesor.<\/li>\n\n\n\n<li><sup>(d)<\/sup> Para alambre de 3.96 mm (5\/32 in.) y menos, el alargamiento y la reducci\u00f3n de \u00e1rea ser\u00e1n de 25 y 40%, respectivamente.<\/li>\n\n\n\n<li><sup>(e)<\/sup> 4 mm (0.156 in.) de di\u00e1metro y m\u00e1s.<\/li>\n\n\n\n<li><sup>(f)<\/sup> Para secciones forjadas de 127 mm (5 in.) y m\u00e1s, la resistencia a la tracci\u00f3n ser\u00e1 de 485 MPa (70 ksi).<\/li>\n\n\n\n<li><sup>(g)<\/sup> Solo para informaci\u00f3n, no es base para aceptaci\u00f3n o rechazo.<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\">Aceros inoxidables austen\u00edticos de alto nitr\u00f3geno<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Los grados de alto nitr\u00f3geno, donde el nitr\u00f3geno reemplaza parte del n\u00edquel para resistencia y para resistencia al picado. Tabla 8 de la fuente.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">UNS<\/th><th class=\"has-text-align-left\" data-align=\"left\">Forma<\/th><th class=\"has-text-align-left\" data-align=\"left\">Condici\u00f3n<\/th><th class=\"has-text-align-left\" data-align=\"left\">De tensi\u00f3n<br>MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">De tensi\u00f3n<br>ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">L\u00edmite el\u00e1stico 0,2 %<br>MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">L\u00edmite el\u00e1stico 0,2 %<br>ksi<\/th><th class=\"has-text-align-left\" data-align=\"left\">Alarg.<br>%<\/th><th class=\"has-text-align-left\" data-align=\"left\">Red. de<br>\u00e1rea, %<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza<br>HRB<\/th><th class=\"has-text-align-left\" data-align=\"left\">ASTM<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20100<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">655<\/td><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20100<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/4 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">860<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20100<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/2 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1030<\/td><td class=\"has-text-align-left\" data-align=\"left\">150<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">110<\/td><td class=\"has-text-align-left\" data-align=\"left\">18<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20100<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">3\/4 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1210<\/td><td class=\"has-text-align-left\" data-align=\"left\">175<\/td><td class=\"has-text-align-left\" data-align=\"left\">930<\/td><td class=\"has-text-align-left\" data-align=\"left\">135<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20100<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Totalmente duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">1280<\/td><td class=\"has-text-align-left\" data-align=\"left\">185<\/td><td class=\"has-text-align-left\" data-align=\"left\">965<\/td><td class=\"has-text-align-left\" data-align=\"left\">140<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 202<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20200<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 202<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20200<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">260<\/td><td class=\"has-text-align-left\" data-align=\"left\">38<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 202<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20200<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/4 duro<\/td><td class=\"has-text-align-left\" data-align=\"left\">860<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 660<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 205<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20500<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">790<\/td><td class=\"has-text-align-left\" data-align=\"left\">115<\/td><td class=\"has-text-align-left\" data-align=\"left\">450<\/td><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">10 m\u00e1x<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 50<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20910<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 50<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20910<\/td><td class=\"has-text-align-left\" data-align=\"left\">W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 50<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20910<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">725<\/td><td class=\"has-text-align-left\" data-align=\"left\">105<\/td><td class=\"has-text-align-left\" data-align=\"left\">415<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 50<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20910<\/td><td class=\"has-text-align-left\" data-align=\"left\">P<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tenelon criog\u00e9nico<\/td><td class=\"has-text-align-left\" data-align=\"left\">S21460<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">725<\/td><td class=\"has-text-align-left\" data-align=\"left\">105<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 216 y 216L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S21600, S21603<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">415<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipos 216 y 216L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S21600, S21603<\/td><td class=\"has-text-align-left\" data-align=\"left\">P<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">345<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 40<\/td><td class=\"has-text-align-left\" data-align=\"left\">S21900<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">345<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">21-6-9 LC (XM-11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">S21904<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W, perfiles<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">345<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">21-6-9 LC (XM-11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">S21904<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">415<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">21-6-9 LC (XM-11)<\/td><td class=\"has-text-align-left\" data-align=\"left\">S21904<\/td><td class=\"has-text-align-left\" data-align=\"left\">P<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">345<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 666<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 33<\/td><td class=\"has-text-align-left\" data-align=\"left\">S24000<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 33<\/td><td class=\"has-text-align-left\" data-align=\"left\">S24000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">415<\/td><td class=\"has-text-align-left\" data-align=\"left\">60<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 33<\/td><td class=\"has-text-align-left\" data-align=\"left\">S24000<\/td><td class=\"has-text-align-left\" data-align=\"left\">P<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitronic 32<\/td><td class=\"has-text-align-left\" data-align=\"left\">S24100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">690<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">380<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276, A 580<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304N<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30451<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304N<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30451<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 340HN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30452<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">345<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 340HN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30452<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">620<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">345<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 340HN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30452<\/td><td class=\"has-text-align-left\" data-align=\"left\">P<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">585<\/td><td class=\"has-text-align-left\" data-align=\"left\">85<\/td><td class=\"has-text-align-left\" data-align=\"left\">275<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304LN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30453<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304LN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30453<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">515<\/td><td class=\"has-text-align-left\" data-align=\"left\">75<\/td><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">253 MA<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30815<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">87<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">253 MA<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30815<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, shapes<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">87<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">45<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">254 SMO<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31254<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">94<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">44<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">96<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">254 SMO<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31254<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, shapes<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">44<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316N<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31651<\/td><td class=\"has-text-align-left\" data-align=\"left\">B<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316N<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31651<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 m\u00e1x.<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">17-14-4 LN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31726<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">96<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">17-14-4 LN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31726<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, shapes<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 276<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">317LN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31753<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">550<\/td><td class=\"has-text-align-left\" data-align=\"left\">80<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">A 167, A 240<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL 6XN<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08367<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">715<\/td><td class=\"has-text-align-left\" data-align=\"left\">104<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">46<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B691<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL 6XN<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08367<\/td><td class=\"has-text-align-left\" data-align=\"left\">P, Sh, St<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">715<\/td><td class=\"has-text-align-left\" data-align=\"left\">104<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">46<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">100<\/td><td class=\"has-text-align-left\" data-align=\"left\">B688<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL 6XN<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08367<\/td><td class=\"has-text-align-left\" data-align=\"left\">Bridas, accesorios, v\u00e1lvulas, etc.<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">715<\/td><td class=\"has-text-align-left\" data-align=\"left\">104<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">46<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B462<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL 6XN<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08367<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sin costura Pi, T<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">715<\/td><td class=\"has-text-align-left\" data-align=\"left\">104<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">46<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B690<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL 6XN<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08367<\/td><td class=\"has-text-align-left\" data-align=\"left\">Pi soldado<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">715<\/td><td class=\"has-text-align-left\" data-align=\"left\">104<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">46<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B676<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL 6XN<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08367<\/td><td class=\"has-text-align-left\" data-align=\"left\">T soldado<\/td><td class=\"has-text-align-left\" data-align=\"left\">Tratado en soluci\u00f3n y recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">715<\/td><td class=\"has-text-align-left\" data-align=\"left\">104<\/td><td class=\"has-text-align-left\" data-align=\"left\">315<\/td><td class=\"has-text-align-left\" data-align=\"left\">46<\/td><td class=\"has-text-align-left\" data-align=\"left\">30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B676<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AL 6XN<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08367<\/td><td class=\"has-text-align-left\" data-align=\"left\">T soldado<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trabajado en fr\u00edo<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B676<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Cronifer 1925 hMO<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08925<\/td><td class=\"has-text-align-left\" data-align=\"left\">B, W<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">87<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">43<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B649<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Cronifer 1925 hMO<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08925<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sin costura Pi, T<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">87<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">43<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B677<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Cronifer 1925 hMO<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08925<\/td><td class=\"has-text-align-left\" data-align=\"left\">Pi soldado<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">87<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">43<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B673<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Cronifer 1925 hMO<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08925<\/td><td class=\"has-text-align-left\" data-align=\"left\">T soldado<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recocido<\/td><td class=\"has-text-align-left\" data-align=\"left\">600<\/td><td class=\"has-text-align-left\" data-align=\"left\">87<\/td><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">43<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">B674<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Fuente: ASM Handbook, Vol 1 (10th ed.), &#8220;Wrought Stainless Steels&#8221;, Table 8. Los valores son propiedades m\u00ednimas a temperatura ambiente seg\u00fan la forma del producto y la condici\u00f3n.<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li><sup>(a)<\/sup> B, barra; P, placa; Pi, tuber\u00eda; Sh, chapa; St, fleje; T, tubo; W, alambre.<\/li>\n<\/ul>\n\n\n\n<ul class=\"wp-block-list\">\n<li>Los c\u00f3digos de forma de producto son B para barra, P para placa, Sh para chapa, St para fleje y W para alambre. Un tipo puede tener diferentes m\u00ednimos en distintas formas, por lo que el mismo acero aparece m\u00e1s de una vez en la tabla.<\/li>\n\n\n\n<li>Las condiciones de trabajo en fr\u00edo se dan en cuartos de dureza, desde un cuarto de dureza hasta dureza completa. La resistencia a la tracci\u00f3n y el l\u00edmite el\u00e1stico aumentan con la cantidad de trabajo en fr\u00edo y el alargamiento disminuye.<\/li>\n\n\n\n<li>La dureza se da como m\u00e1ximo para las condiciones blandas y a menudo no se especifica para las de trabajo en fr\u00edo, donde los m\u00ednimos de resistencia ya controlan la condici\u00f3n.<\/li>\n<\/ul>\n\n\n\n<h3 id=\"h-table-notes\" class=\"wp-block-heading\">Notas de la tabla<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Dos valores en la tabla de origen parecen defectos de impresi\u00f3n y se reproducen tal como se imprimieron en lugar de corregirse. Al tipo 205 en barra, placa, chapa y fleje se le asigna una dureza de 10 m\u00e1x HRB, cuando la condici\u00f3n recocida de todos los tipos similares se sit\u00faa en 90 HRB o m\u00e1s. La chapa y el fleje de tipo 202 trabajados en fr\u00edo citan ASTM A 660 donde todas las filas vecinas citan A 666. Los tipos 347 y 348 en condici\u00f3n acabada en caliente y recocida no llevan valor de dureza en la tabla de origen, y esa celda se deja en blanco aqu\u00ed en lugar de rellenarse. Los n\u00fameros UNS de los tipos 321 y 321H se imprimen como S32100, 32109 en la fuente y se dan aqu\u00ed como S32100, S32109.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Los valores anteriores son valores m\u00ednimos de aceptaci\u00f3n, no propiedades t\u00edpicas. Una colada se ensaya contra el m\u00ednimo para su forma de producto, por lo que un certificado que muestra 620 MPa de resistencia a la tracci\u00f3n en un tipo con un m\u00ednimo de 515 MPa es normal y no un grado diferente.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Los datos de composici\u00f3n son solo para referencia general. Los valores reales var\u00edan seg\u00fan la norma, la acer\u00eda y el n\u00famero de colada. Confirme con el certificado de ensayo del material (MTC) o contacte con Aobo Steel. El <a href=\"\/es\/martensitic-stainless-steel-properties-chart\/\">tabla de propiedades de aceros inoxidables martens\u00edticos<\/a> cubre las series 410, 420 y 440 de la misma manera.<\/p>\n\n\n\n<h2 id=\"h-austenitic-against-martensitic\" class=\"wp-block-heading\">Austen\u00edtico frente a martens\u00edtico<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">La serie 300 no puede endurecerse por tratamiento t\u00e9rmico y estos m\u00ednimos se alcanzan mediante recocido o trabajo en fr\u00edo. Los <a href=\"\/es\/martensitic-stainless-steel-properties-chart\/\">grados martens\u00edticos<\/a> se endurecen mediante temple y revenido en su lugar.<\/p>\n\n\n\n<h2 id=\"h-yield-is-quoted-at-0-2-offset\" class=\"wp-block-heading\">El l\u00edmite el\u00e1stico se cita con un desplazamiento del 0,2 %<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">El acero inoxidable austen\u00edtico no tiene un l\u00edmite el\u00e1stico definido, por lo que la norma utiliza la tensi\u00f3n que produce un 0,2 % de deformaci\u00f3n permanente. Dos proveedores que citan el l\u00edmite el\u00e1stico sin indicar qu\u00e9 desplazamiento no est\u00e1n citando el mismo n\u00famero.<\/p>\n\n\n\n<h2 id=\"h-cold-work-instead-of-alloy\" class=\"wp-block-heading\">Trabajo en fr\u00edo en lugar de aleaci\u00f3n<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">El 301 en un cuarto de dureza alcanza aproximadamente el doble del l\u00edmite el\u00e1stico del 301 recocido sin cambios en la composici\u00f3n qu\u00edmica. Ese es el aumento de resistencia m\u00e1s econ\u00f3mico disponible en la serie 300 y la raz\u00f3n por la que los grados para resortes y flejes se piden trabajados en fr\u00edo.<\/p>\n\n\n\n<h3 id=\"h-related-reference-pages\" class=\"wp-block-heading\">P\u00e1ginas de referencia relacionadas<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"\/es\/stainless-steel-composition-chart\/\">tabla de composici\u00f3n del acero inoxidable<\/a> \u00b7 <a href=\"\/es\/martensitic-stainless-steel-properties-chart\/\">Tabla de propiedades de aceros inoxidables martens\u00edticos<\/a> \u00b7 <a href=\"\/es\/stainless-steel-physical-properties-chart\/\">Tabla de propiedades f\u00edsicas del acero inoxidable<\/a> \u00b7 <a href=\"\/es\/420-stainless-steel\/\">acero inoxidable 420<\/a> \u00b7 <a href=\"\/es\/440c-stainless-steel\/\">acero inoxidable 440C<\/a> \u00b7 <a href=\"\/es\/4cr13-stainless-steel\/\">acero inoxidable 4Cr13<\/a> \u00b7 <a href=\"\/es\/stainless-steels\/\">Descripci\u00f3n general de los aceros inoxidables<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fuente: ASM Handbook, Vol 1 (10.\u00aa ed.), &#8220;Wrought Stainless Steels&#8221;, Tabla 7. Los valores son propiedades m\u00ednimas a temperatura ambiente seg\u00fan la forma de producto y la condici\u00f3n.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Propiedades mec\u00e1nicas del acero inoxidable austen\u00edtico, PDF para imprimir<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Tres p\u00e1ginas A4 con los valores m\u00ednimos de resistencia a la tracci\u00f3n y l\u00edmite el\u00e1stico, alargamiento, reducci\u00f3n de \u00e1rea y dureza de 147 filas de tipo, forma de producto y estado, la especificaci\u00f3n ASTM indicada en cada fila y nuestros datos de contacto. El PDF est\u00e1 en ingl\u00e9s.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Austenitic-Stainless-Mechanical-Properties.pdf\">Descargar PDF, 707 KB<\/a><\/div>\n<\/div>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Mechanical Properties of Austenitic Stainless Steels Minimum room-temperature tensile and yield strength, elongation, reduction in area and hardness for the wrought austenitic stainless steels, quoted for each product form and condition with the ASTM specification that carries the requirement. A minimum is the floor a heat has to clear, so a certificate usually shows more. [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-19422","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Austenitic Stainless Steel Properties Chart | Aobo Steel<\/title>\n<meta name=\"description\" content=\"Minimum tensile and yield strength, elongation, reduction of area and hardness for the wrought 200 and 300 series austenitic stainless steels, by product form and condition.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/es\/austenitic-stainless-steel-mechanical-properties\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Austenitic Stainless Steel Mechanical Properties Chart\" \/>\n<meta property=\"og:description\" content=\"Minimum tensile and yield strength, elongation, reduction of area and hardness for the wrought 200 and 300 series austenitic stainless steels, by product form and condition.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/es\/austenitic-stainless-steel-mechanical-properties\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-16T02:28:40+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"18 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/austenitic-stainless-steel-mechanical-properties\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/austenitic-stainless-steel-mechanical-properties\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Austenitic Stainless Steel Mechanical Properties Chart\",\"datePublished\":\"2026-09-21T05:28:57+00:00\",\"dateModified\":\"2026-10-16T02:28:40+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/austenitic-stainless-steel-mechanical-properties\\\/\"},\"wordCount\":2514,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"es\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/austenitic-stainless-steel-mechanical-properties\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/austenitic-stainless-steel-mechanical-properties\\\/\",\"name\":\"Austenitic Stainless Steel Properties Chart | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-21T05:28:57+00:00\",\"dateModified\":\"2026-10-16T02:28:40+00:00\",\"description\":\"Minimum tensile and yield strength, elongation, reduction of area and hardness for the wrought 200 and 300 series austenitic stainless steels, by product form and condition.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/austenitic-stainless-steel-mechanical-properties\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/austenitic-stainless-steel-mechanical-properties\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/austenitic-stainless-steel-mechanical-properties\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Austenitic Stainless Steel Mechanical Properties Chart\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/es\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tabla de propiedades del acero inoxidable austen\u00edtico | Aobo Steel","description":"Resistencia m\u00ednima a la tracci\u00f3n y l\u00edmite el\u00e1stico, alargamiento, reducci\u00f3n de \u00e1rea y dureza para los aceros inoxidables austen\u00edticos forjados de las series 200 y 300, por forma de producto y condici\u00f3n.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/es\/austenitic-stainless-steel-mechanical-properties\/","og_locale":"es_ES","og_type":"article","og_title":"Austenitic Stainless Steel Mechanical Properties Chart","og_description":"Minimum tensile and yield strength, elongation, reduction of area and hardness for the wrought 200 and 300 series austenitic stainless steels, by product form and condition.","og_url":"https:\/\/aobosteel.com\/es\/austenitic-stainless-steel-mechanical-properties\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-16T02:28:40+00:00","twitter_card":"summary_large_image","twitter_misc":{"Tiempo de lectura":"18 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/austenitic-stainless-steel-mechanical-properties\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/austenitic-stainless-steel-mechanical-properties\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Austenitic Stainless Steel Mechanical Properties Chart","datePublished":"2026-09-21T05:28:57+00:00","dateModified":"2026-10-16T02:28:40+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/austenitic-stainless-steel-mechanical-properties\/"},"wordCount":2514,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"es"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/austenitic-stainless-steel-mechanical-properties\/","url":"https:\/\/aobosteel.com\/austenitic-stainless-steel-mechanical-properties\/","name":"Tabla de propiedades del acero inoxidable austen\u00edtico | Aobo Steel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-21T05:28:57+00:00","dateModified":"2026-10-16T02:28:40+00:00","description":"Resistencia m\u00ednima a la tracci\u00f3n y l\u00edmite el\u00e1stico, alargamiento, reducci\u00f3n de \u00e1rea y dureza para los aceros inoxidables austen\u00edticos forjados de las series 200 y 300, por forma de producto y condici\u00f3n.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/austenitic-stainless-steel-mechanical-properties\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/austenitic-stainless-steel-mechanical-properties\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/austenitic-stainless-steel-mechanical-properties\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Austenitic Stainless Steel Mechanical Properties Chart"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Mechanical Properties of Austenitic Stainless Steels Minimum room-temperature tensile and yield strength, elongation, reduction in area and hardness for the wrought austenitic stainless steels, quoted for each product form and condition with the ASTM specification that carries the requirement. A minimum is the floor a heat has to clear, so a certificate usually shows more.&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Mechanical Properties of Austenitic Stainless Steels Minimum room-temperature tensile and yield strength, elongation, reduction in area and hardness for the wrought austenitic stainless steels, quoted for each product form and condition with the ASTM specification that carries the requirement. A minimum is the floor a heat has to clear, so a certificate usually shows more.&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/19422","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/comments?post=19422"}],"version-history":[{"count":11,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/19422\/revisions"}],"predecessor-version":[{"id":23041,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/19422\/revisions\/23041"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/media?parent=19422"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}