{"id":18236,"date":"2026-09-13T15:16:27","date_gmt":"2026-09-13T07:16:27","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=18236"},"modified":"2026-10-26T07:50:48","modified_gmt":"2026-10-25T23:50:48","slug":"stainless-steel-composition-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/es\/stainless-steel-composition-chart\/","title":{"rendered":"Tabla de composici\u00f3n del acero inoxidable para todos los grados AISI"},"content":{"rendered":"<h1 class=\"wp-block-heading has-text-align-center\" style=\"font-size:36px\">tabla de composici\u00f3n del acero inoxidable<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">L\u00edmites de composici\u00f3n qu\u00edmica para los tipos est\u00e1ndar de acero inoxidable AISI &mdash; las familias austen\u00edtica, ferr\u00edtica, d\u00faplex, martens\u00edtica y endurecible por precipitaci\u00f3n. Los rangos est\u00e1n en porcentaje en peso; un valor \u00fanico es un m\u00e1ximo a menos que se indique &ldquo;min&rdquo;.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>peso %<\/strong> todos los valores<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>16.0-18.0<\/strong> rango de \u2013 a<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>0,15 min<\/strong> contenido m\u00ednimo<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>0.045<\/strong> l\u00edmite m\u00e1ximo<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>&mdash;<\/strong> no especificado<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>(a)&ndash;(b)<\/strong> nota<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">UNS<\/th><th class=\"has-text-align-left\" data-align=\"left\">C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mn<\/th><th class=\"has-text-align-left\" data-align=\"left\">Si<\/th><th class=\"has-text-align-left\" data-align=\"left\">Cr<\/th><th class=\"has-text-align-left\" data-align=\"left\">Ni<\/th><th class=\"has-text-align-left\" data-align=\"left\">P<\/th><th class=\"has-text-align-left\" data-align=\"left\">S<\/th><th class=\"has-text-align-left\" data-align=\"left\">Otro<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Tipos austen\u00edticos<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">201<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20100<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.5-7.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5-5.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">202<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.5-10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0-6.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">205<\/td><td class=\"has-text-align-left\" data-align=\"left\">S20500<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12-0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.0-15.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.5-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0-1.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.32-0.40 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">301<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30100<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.0-8.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">302<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">302B<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30215<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0-3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">303<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30300<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.6 Mo <sup>(b)<\/sup><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">303Se<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30323<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min Se<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">304<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0-20.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-10.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">304H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30409<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04-0.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0-20.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-10.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30403<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0-20.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-12.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">304LN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30453<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0-20.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-12.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.10-0.16 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">302Cu<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30430<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0-4.0 Cu<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">304N<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30451<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0-20.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.0-10.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.10-0.16 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">305<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30500<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.5-13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">308<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30800<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.0-21.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0-12.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">309<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30900<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.0-24.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0-15.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">309S<\/td><td class=\"has-text-align-left\" data-align=\"left\">S30908<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">22.0-24.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0-15.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31000<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.0-26.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.0-22.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">310S<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31008<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">24.0-26.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.0-22.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">314<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5-3.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.0-26.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">19.0-22.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31600<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0-3.0 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316F<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31620<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,10 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.75-2.5 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31609<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04-0.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0-3.0 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31603<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0-3.0 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316LN<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31653<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0-3.0 Mo; 0.10-0.16 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">316N<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31651<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0-3.0 Mo; 0.10-0.16 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">317<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31700<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0-20.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0-15.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0-4.0 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">317L<\/td><td class=\"has-text-align-left\" data-align=\"left\">S31703<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0-20.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.0-15.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0-4.0 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">321<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32100<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.0-12.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">5 \u00d7 %C min Ti<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">321H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32109<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04-0.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.0-12.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">5 \u00d7 %C min Ti<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">330<\/td><td class=\"has-text-align-left\" data-align=\"left\">N08330<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75-1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-20.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">34.0-37.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">347<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34700<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.0-13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">10 \u00d7 %C min Nb<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">347H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34709<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04-0.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.0-13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">8 \u00d7 %C min &#8211; 1,0 m\u00e1x Nb<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">348<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34800<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.0-13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,2 Co; 10 \u00d7 %C min Nb; 0,10 Ta<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">348H<\/td><td class=\"has-text-align-left\" data-align=\"left\">S34809<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04-0.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.0-13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,2 Co; 8 \u00d7 %C min &#8211; 1,0 m\u00e1x Nb; 0,10 Ta<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">384<\/td><td class=\"has-text-align-left\" data-align=\"left\">S38400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.0-17.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Tipos ferr\u00edticos<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">405<\/td><td class=\"has-text-align-left\" data-align=\"left\">S40500<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5-14.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.10-0.30 Al<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">409<\/td><td class=\"has-text-align-left\" data-align=\"left\">S40900<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.08<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.5-11.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.045<\/td><td class=\"has-text-align-left\" data-align=\"left\">6 \u00d7 %C min &#8211; 0,75 m\u00e1x Ti<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">429<\/td><td class=\"has-text-align-left\" data-align=\"left\">S42900<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.0-16.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">430<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43000<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">430F<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43020<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.6 Mo <sup>(b)<\/sup><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">430FSe<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43023<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min Se<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">434<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75-1.25 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">436<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43600<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,75-1,25 Mo; 5 \u00d7 %C min &#8211; 0,70 m\u00e1x Nb<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">439<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43035<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.07<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0-19.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 Al; 12 \u00d7 %C min &#8211; 1,10 Ti<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">442<\/td><td class=\"has-text-align-left\" data-align=\"left\">S44200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">18.0-23.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">444<\/td><td class=\"has-text-align-left\" data-align=\"left\">S44400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.5-19.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">1,75-2,50 Mo; 0,025 N; 0,2 + 4 (%C + %N) min &#8211; 0,8 m\u00e1x (Ti + Nb)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">446<\/td><td class=\"has-text-align-left\" data-align=\"left\">S44600<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.0-27.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Tipo d\u00faplex (ferr\u00edtico-austen\u00edtico)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">329<\/td><td class=\"has-text-align-left\" data-align=\"left\">S32900<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">23.0-28.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.50-5.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.040<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.030<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00-2.00 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Tipos martens\u00edticos<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">403<\/td><td class=\"has-text-align-left\" data-align=\"left\">S40300<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5-13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/es\/410-stainless-steel-heat-treatment\/\">410<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">S41000<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5-13.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">414<\/td><td class=\"has-text-align-left\" data-align=\"left\">S41400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5-13.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25-2.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/es\/416-stainless-steel-heat-treatment\/\">416<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">S41600<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.6 Mo <sup>(b)<\/sup><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">416Se<\/td><td class=\"has-text-align-left\" data-align=\"left\">S41623<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min Se<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">420<\/td><td class=\"has-text-align-left\" data-align=\"left\">S42000<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">420F<\/td><td class=\"has-text-align-left\" data-align=\"left\">S42020<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0-14.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">0,15 min<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.6 Mo <sup>(b)<\/sup><\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">422<\/td><td class=\"has-text-align-left\" data-align=\"left\">S42200<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20-0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5-13.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5-1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75-1.25 Mo; 0.75-1.25 W; 0.15-0.3 V<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">431<\/td><td class=\"has-text-align-left\" data-align=\"left\">S43100<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.0-17.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25-2.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/es\/440a-stainless-steel-heat-treatment\/\">440A<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">S44002<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.60-0.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/es\/440b-stainless-steel-heat-treatment\/\">440B<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">S44003<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75-0.95<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">440C<\/td><td class=\"has-text-align-left\" data-align=\"left\">S44004<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.95-1.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">&mdash;<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75 Mo<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"10\">Tipos endurecibles por precipitaci\u00f3n<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">PH 13-8 Mo<\/td><td class=\"has-text-align-left\" data-align=\"left\">S13800<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.20<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.25-13.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.5-8.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.01<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.008<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0-2.5 Mo; 0.90-1.35 Al; 0.01 N<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">15-5 PH<\/td><td class=\"has-text-align-left\" data-align=\"left\">S15500<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.07<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.0-15.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.5-5.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5-4.5 Cu; 0.15-0.45 Nb<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">17-4 PH<\/td><td class=\"has-text-align-left\" data-align=\"left\">S17400<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.07<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.5-17.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0-5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.0-5.0 Cu; 0.15-0.45 Nb<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">17-7 PH<\/td><td class=\"has-text-align-left\" data-align=\"left\">S17700<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.09<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">16.0-18.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5-7.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.75-1.5 Al<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<ul class=\"wp-block-list\">\n<li><sup>(a)<\/sup> Los valores \u00fanicos son valores m\u00e1ximos a menos que se indique lo contrario (un valor seguido de &ldquo;min&rdquo; es un m\u00ednimo).<\/li>\n\n<li><sup>(b)<\/sup> Opcional.<\/li>\n<\/ul>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-1b2ccf01 wp-block-group-is-layout-constrained\" style=\"border-radius:10px;background-color:#f4f8ff;margin-bottom:22px;padding-top:22px;padding-right:26px;padding-bottom:20px;padding-left:26px\">\n\n<h3 class=\"wp-block-heading\" style=\"font-size:22px\">Notas de la tabla<\/h3>\n\n\n<p class=\"wp-block-paragraph\">La columna &ldquo;Otros&rdquo; indica elementos adicionales especificados &mdash; nitr\u00f3geno, cobre, titanio, niobio, aluminio, molibdeno, selenio y tungsteno &mdash; tal como se imprimen en la fuente.<\/p>\n\n\n<p class=\"wp-block-paragraph\">El carbono del tipo 420 es un m\u00ednimo (0,15 % min); el carbono real var\u00eda seg\u00fan la colada, por lo que debe verificarse el certificado de la acer\u00eda cuando la dureza sea importante. El UNS S30430 aparece en esta tabla bajo su designaci\u00f3n AISI 302Cu; algunas referencias listan la misma composici\u00f3n como 304Cu.<\/p>\n\n\n<p class=\"wp-block-paragraph\">Los l\u00edmites de composici\u00f3n son valores de an\u00e1lisis de colada de la fuente. Pueden aplicarse tolerancias de an\u00e1lisis del producto &mdash; confirme la especificaci\u00f3n aplicable con su proveedor antes de realizar el pedido.<\/p>\n\n<\/div>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-1b2ccf01 wp-block-group-is-layout-constrained\" style=\"border-radius:10px;background-color:#f4f8ff;margin-bottom:22px;padding-top:22px;padding-right:26px;padding-bottom:20px;padding-left:26px\">\n\n<h3 class=\"wp-block-heading\" style=\"font-size:22px\">P\u00e1ginas de referencia relacionadas<\/h3>\n\n\n<p class=\"wp-block-paragraph\"><a href=\"\/es\/stainless-steels\/\">Descripci\u00f3n general de los aceros inoxidables<\/a> \u00b7 <a href=\"\/es\/420-stainless-steel\/\">acero inoxidable 420<\/a> \u00b7 <a href=\"\/es\/420-stainless-steel-heat-treatment\/\">Tratamiento t\u00e9rmico del acero inoxidable 420<\/a> \u00b7 <a href=\"\/es\/440c-stainless-steel\/\">acero inoxidable 440C<\/a> \u00b7 <a href=\"\/es\/440c-stainless-steel-properties\/\">Propiedades del acero inoxidable 440C<\/a> \u00b7 <a href=\"\/es\/440c-stainless-steel-heat-treatment\/\">Tratamiento t\u00e9rmico del acero inoxidable 440C<\/a> \u00b7 <a href=\"\/es\/4cr13-stainless-steel\/\">acero inoxidable 4Cr13<\/a> \u00b7 <a href=\"\/es\/9cr18mo-stainless-steel\/\">Acero inoxidable 9Cr18Mo<\/a> \u00b7 <a href=\"\/es\/tool-steel-composition-chart\/\">Tabla de composici\u00f3n del acero para herramientas<\/a> \u00b7 <a href=\"\/es\/95cr18-stainless-steel-3\/\">Acero inoxidable 95Cr18 (9Cr18)<\/a> \u00b7 <a href=\"\/es\/stainless-steel-physical-properties-chart\/\">Tabla de propiedades f\u00edsicas del acero inoxidable<\/a> \u00b7 <a href=\"\/es\/austenitic-stainless-steel-mechanical-properties\/\">Propiedades mec\u00e1nicas del acero inoxidable austen\u00edtico<\/a><\/p>\n\n\n<p class=\"wp-block-paragraph\">Fuente: ASM Handbook, Volumen 1 &mdash; Properties and Selection: Irons, Steels, and High-Performance Alloys, Tabla 2 &ldquo;Compositions of standard stainless steels&rdquo; (10.\u00aa ed.). Datos de referencia para comparaci\u00f3n &mdash; verifique la norma aplicable antes de realizar el pedido.<\/p>\n\n\n\n<\/div>","protected":false},"excerpt":{"rendered":"<p>Stainless Steel Composition Chart Chemical composition limits for the standard AISI stainless steel types &mdash; the austenitic, ferritic, duplex, martensitic and precipitation-hardening families. Ranges are in weight percent; a single value is a maximum unless marked &ldquo;min&rdquo;. wt % all values 16.0-18.0 from&ndash;to range 0.15 min minimum content 0.045 maximum limit &mdash; not specified (a)&ndash;(b) [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-18236","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Stainless Steel Composition Chart for All AISI Grades - AoboSteel<\/title>\n<meta name=\"description\" content=\"Compare chemical composition limits for austenitic, ferritic, duplex, martensitic, and PH stainless steels across all standard AISI grades.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/es\/stainless-steel-composition-chart\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Stainless Steel Composition Chart for All AISI Grades\" \/>\n<meta property=\"og:description\" content=\"Compare chemical composition limits for austenitic, ferritic, duplex, martensitic, and PH stainless steels across all standard AISI grades.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/es\/stainless-steel-composition-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-25T23:50:48+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"5 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-composition-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-composition-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Stainless Steel Composition Chart for All AISI Grades\",\"datePublished\":\"2026-09-13T07:16:27+00:00\",\"dateModified\":\"2026-10-25T23:50:48+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-composition-chart\\\/\"},\"wordCount\":694,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"es\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-composition-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-composition-chart\\\/\",\"name\":\"Stainless Steel Composition Chart for All AISI Grades - AoboSteel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-13T07:16:27+00:00\",\"dateModified\":\"2026-10-25T23:50:48+00:00\",\"description\":\"Compare chemical composition limits for austenitic, ferritic, duplex, martensitic, and PH stainless steels across all standard AISI grades.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-composition-chart\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-composition-chart\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-composition-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Stainless Steel Composition Chart for All AISI Grades\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/es\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tabla de composici\u00f3n del acero inoxidable para todos los grados AISI - AoboSteel","description":"Compare los l\u00edmites de composici\u00f3n qu\u00edmica de los aceros inoxidables austen\u00edticos, ferr\u00edticos, d\u00faplex, martens\u00edticos y PH en todos los grados est\u00e1ndar AISI.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/es\/stainless-steel-composition-chart\/","og_locale":"es_ES","og_type":"article","og_title":"Stainless Steel Composition Chart for All AISI Grades","og_description":"Compare chemical composition limits for austenitic, ferritic, duplex, martensitic, and PH stainless steels across all standard AISI grades.","og_url":"https:\/\/aobosteel.com\/es\/stainless-steel-composition-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-25T23:50:48+00:00","twitter_card":"summary_large_image","twitter_misc":{"Tiempo de lectura":"5 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/stainless-steel-composition-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/stainless-steel-composition-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Stainless Steel Composition Chart for All AISI Grades","datePublished":"2026-09-13T07:16:27+00:00","dateModified":"2026-10-25T23:50:48+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/stainless-steel-composition-chart\/"},"wordCount":694,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"es"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/stainless-steel-composition-chart\/","url":"https:\/\/aobosteel.com\/stainless-steel-composition-chart\/","name":"Tabla de composici\u00f3n del acero inoxidable para todos los grados AISI - AoboSteel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-13T07:16:27+00:00","dateModified":"2026-10-25T23:50:48+00:00","description":"Compare los l\u00edmites de composici\u00f3n qu\u00edmica de los aceros inoxidables austen\u00edticos, ferr\u00edticos, d\u00faplex, martens\u00edticos y PH en todos los grados est\u00e1ndar AISI.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/stainless-steel-composition-chart\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/stainless-steel-composition-chart\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/stainless-steel-composition-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Stainless Steel Composition Chart for All AISI Grades"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Stainless Steel Composition Chart Chemical composition limits for the standard AISI stainless steel types &mdash; the austenitic, ferritic, duplex, martensitic and precipitation-hardening families. Ranges are in weight percent; a single value is a maximum unless marked &ldquo;min&rdquo;. wt % all values 16.0-18.0 from&ndash;to range 0.15 min minimum content 0.045 maximum limit &mdash; not specified (a)&ndash;(b)&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/es\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Stainless Steel Composition Chart Chemical composition limits for the standard AISI stainless steel types &mdash; the austenitic, ferritic, duplex, martensitic and precipitation-hardening families. Ranges are in weight percent; a single value is a maximum unless marked &ldquo;min&rdquo;. wt % all values 16.0-18.0 from&ndash;to range 0.15 min minimum content 0.045 maximum limit &mdash; not specified (a)&ndash;(b)&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/18236","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/comments?post=18236"}],"version-history":[{"count":13,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/18236\/revisions"}],"predecessor-version":[{"id":24539,"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/pages\/18236\/revisions\/24539"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/es\/wp-json\/wp\/v2\/media?parent=18236"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}