GCr15 Steel | 52100
AOBO STEEL – Trusted Global Tool Steel Supplier
GCr15 steel is a widely used high-carbon chromium bearing steel and is also considered a low-alloy cold work mold steel. It is a representative grade among high-carbon chromium-bearing steels. This steel can be either water or oil quenched, depending on the application and desired properties.
1. Chemical Composition(GB / T 18254—2002)
| C | Si | Mn | Cr | P | S | PROTI |
| 0.95 ~ 1.05 | 0.15 ~ 0.35 | 0.25 ~ 0.45 | 1.40 ~ 1.65 | ≤0.025 | ≤0.025 | — |
2. GCr15 Steel Critical Point Temperature
| Kritický bod | Klimatizace1 | Klimatizacecm | Ar1 | paní |
| Temperature (Approx. Value)/°C | 745 | 900 | 700 | 246 |
3. GCr15 Steel Forging Process Specification
| Položka | Teplota ohřevu/°C | Počáteční teplota kování/°C | Konečná teplota kování/°C | Chlazení |
| Ocelový ingot | 1150 ~ 1200 | 1100 ~ 1150 | 800 ~ 880 | First air-cool to 700°C, then pit-cool |
| Ocelový předvalek | 1080 ~ 1120 | 1050 ~ 1100 | 800 ~ 850 | First air-cool to 700°C, then pit-cool |
4. GCr15 Steel Heat Treatment Process Specification
4.1 Předehřívání
| Předběžný plán tepelného zpracování | Procesní parametry |
| Izotermické žíhání po kování | Slowly heat to 770 ~ 790°C, hold for 1 ~ 2h; furnace cool to 680 ~ 700°C, hold for 3 ~ 4h, then furnace cool to below 550°C and air cool. Hardness: 180 ~ 229HBW. |
| High-Temperature Tempering | Heating temperature: 600 ~ 700°C, hold for 2 ~ 3h; furnace cool or air cool. Hardness: 187 ~ 229HBW. Mainly used to eliminate machining stress before quenching. |
| Normalizace | Heating temperature: 930 ~ 950°C, air cool. Hardness: 302 ~ 388HBW. Used to refine the grains of overheated steel and eliminate network carbides. |
| Kalení a temperování | Quenching temperature: 840 ~ 860°C, oil cool; tempering temperature: 660 ~ 680°C, furnace cool or air cool. Hardness: 197 ~ 217HBW. |
4.2 Kalení
| Quenching Process Plan | Procesní parametry |
| Conventional Quenching Process | Heating temperature: 830 ~ 850°C, oil cool. Hardness: 62 ~ 65HRC. |
| Izotermický proces kalení | Heating temperature: 830 ~ 850°C, isothermal quenching at 240 ~ 300°C. Tempering temperature: 180 ~ 200°C. Hardness: 58 ~ 62HRC. |
Poznámka: To save energy and time, the residual heat from forging can be used for the isothermal quenching process to replace spheroidizing annealing.
Ultra-fine processing of carbides.
Carbide Super-refinement Process
| Proces tepelného zpracování | Procesní parametry |
| Super-refinement Treatment | Solution temperature is 1050°C, followed by isothermal treatment in a salt bath at 300 ~ 350°C to obtain a lower bainite structure. The tempering temperature is around 720°C with a holding time of 2h, but the hardness is too high, leading to difficult machining. An alternative is a short-time spheroidizing process: heat to 720°C and hold for one hour, then raise the temperature to 780°C and hold for one hour, then cool back to 720°C and hold for another one hour. Finally, in furnace cooled to 500°C before removing. This process can obtain ultra-fine spheroidized carbides. |
4.3 Temperování
Tempering Process Specification
| Teplota ohřevu/°C | Způsob chlazení | Tvrdost HRC |
| 150 ~ 190 | Oil cool or air cool | 58 ~ 62 |
Tempering Temperature and Hardness
| Teplota popouštění/°C | Netemperovaný | 200 | 300 | 400 | 500 | 550 | 600 | 650 |
| Tvrdost HRC | 62 | 61 | 56 | 49 | 40 | 36 | 31 | 28 |
Poznámka: Oil quenched at 830°C, tempered for two hours.

Please fill out the following contact form to receive the best quotation for GCr15 steel.
5. Mechanické vlastnosti
GCr15 is a special steel for bearings. It has good hardenability, hardness, and wear resistance, high contact fatigue strength, and good dimensional stability during quenching and tempering. Tools and molds made with it have high toughness and wear resistance after low-temperature tempering, which can significantly extend their service life.
Relationship between Quenching Temperature, Microstructure, and Performance
| Teplota kalení/°C | Mass Fraction of Carbon in Martensite (%) | Retained Austenite Content (volume fraction, %) | Tvrdost HRC | Bending Strength σbb/MPa | Impact Toughness αK /(J/cm²) |
| 820 | 0.41, Mainly lath martensite | — | 62.8 | 3234 | 6.67 |
| 835 | 0.49, Mainly lath martensite | 10.40 | 63.7 | 2724 | 5.19 |
| 845 | 0.52, Mixture of lath and acicular martensite | 14.70 | 64.1 | 3420 | 5.19 |
| 855 | 0.55, Mixture of lath and acicular martensite | — | 64.9 | 3263 | 3.53 |
| 865 | 0.59, Mixture of lath and acicular martensite | 16.90 | 65.1 | 2960 | 3.43 |
| 875 | 0.67, Mainly acicular martensite | 21.20 | 65.4 | 2739 | 2.55 |
| 885 | 0.67, Mainly acicular martensite | — | 65.3 | 2450 | 2.45 |
Poznámka: Tempered at 160°C.
6. Aplikace
- Bearings: Its primary and most widespread application is in the manufacturing of various types of bearings, including races, steel balls, tapered rollers, cylindrical rollers, spherical rollers, and needles.
- Molds and Dies (Cold Work): It is frequently used for cold stamping dies, cold heading dies, drawing dies, extrusion dies, and cutting dies/blades. It’s also suitable for plastic molds, especially those requiring high wear resistance, strength, and ability to handle high loads, and for other molds like rolling dies and powder metallurgy dies.
- Precision Measuring Tools: GCr15 is a preferred material for precision measuring instruments such as gauge blocks, plug gauges, and thread ring gauges.
- Machine Parts: It’s utilized in various machine components, including guide pillars and guide bushings, diesel engine injectors, and precision lead screws.
- Other Applications: It’s also used for spring collets and as a material for general cutting tools.
7. Equivalent Material
FAQ
GCr15 steel is a high-carbon chromium bearing steel and a low-alloy cold work mold steel. It is widely used due to its excellent hardness, wear resistance, and high contact fatigue performance after heat treatment.
After quenching, GCr15 steel typically achieves a hardness of ≥62 HRC, 61-65 HRC, or ≥63 HRC. After standard low-temperature tempering (150-190°C), its hardness generally ranges from 58-62 HRC to 61-65 HRC. For instance, GCr15, when oil quenched from 845°C and tempered at 150°C, can reach 61-65 HRC.
GCr15 and 52100 steel are essentially the same material, serving as direct equivalents under different international standards. GCr15 is the Chinese designation, while 52100 is the American ASTM (American Society for Testing and Materials) designation.
Get a Competitive Quote for GCr15 Steel
With over 20 years of forging expertise, Aobo Steel is your trusted partner for high-performance GCr15 steel. We provide not just materials, but solutions. Leverage our deep industry knowledge and reliable supply chain for your project’s success.
✉ Kontaktujte nás vyplněním níže uvedeného formuláře.
Prozkoumejte naše další produkty
D2/1.2379/SKD11
D3/1.2080/SKD1
D6/1,2436/SKD2
A2/1.23663/SKD12
O1/1.2510/SKS3
O2/1,2842
S1/1,2550
S7/1,2355
DC53
H13/1.2344/SKD61
H11/1.2343/SKD6
H21/1,2581/SKD7
L6/1.2714/SKT4
M2/1.3343/SKH51
M35/1.3243/SKH55
M42/1.3247/SKH59
P20/1,2311
P20+Ni/1,2738
420/1.2083/2Cr13
422 z nerezové oceli
Ložisková ocel 52100
Nerezová ocel 440C
4140/42CrMo4/SCM440
4340/34CrNiMo6/1,6582
4130
5140/42Cr4/SCR440
SCM415