Nástrojová ocel Cr12MoV pro práci za studena
AOBO STEEL – Důvěryhodný globální dodavatel nástrojové oceli
Cr12MoV tool steel is a high-carbon, high-chromium ledeburite cold work tool steel with high hardness, wear resistance, and minimal quenching deformation. This steel grade is an improved version of Nástrojová ocel Cr12, with the addition of molybdenum (Mo) and vanadium (V) elements to enhance its performance characteristics.
1. Composition of Cr12MoV Steel(GB/ T 1299—2000)
| C | Si | Mn | Cr | PROTI | Mo | S | P |
|---|---|---|---|---|---|---|---|
| 1.45 ~ 1.70 | ≤0,40 | ≤0,40 | 11.00 ~ 12.50 | 0.15 ~ 0.30 | 0.40 ~ 0.60 | ≤0,030 | ≤0,030 |
2. Properties of Cr12MoV Steel
Teplota kritického bodu
| Kritický bod | Ac1 | Ac₃ | Ar₁ | paní |
|---|---|---|---|---|
| Teplota / °C | 810 | 1200 | 760 | 185 |
Lineární expanzní koeficient
| Teplota / °C | Linear Expansion Coefficient α / (10⁻⁶ °C⁻¹) |
|---|---|
| 20 ~ 100 | 10.9 |
| 20 ~ 400 | 11.4 |
| 20 ~ 600 | 12.2 |
Cr12MoV is a high-carbon, high-chromium, high-hardenability ledeburitic steel. It is characterized by high hardness, good impact toughness, high hardenability, and low distortion upon quenching.
For cross-sectional dimensions up to 400mm, it can be fully through-hardened. Furthermore, it maintains good hardness and wear resistance at elevated temperatures in the range of 300~400 °C.
With minimal volumetric change during quenching and excellent overall mechanical properties, Cr12MoV is considered one of the representative steel grades for high-end cold work tooling materials.
3. Forging Process Specification of Cr12MoV Steel
| Položka | Heating Temp. / °C | Initial Forging Temp. / °C | Final Forging Temp. / °C | Způsob chlazení |
|---|---|---|---|---|
| Ingot | 1100 ~ 1150 | 1050 ~ 1100 | 850 ~ 900 | Slow cooling (pit or sand cooling) |
| Sochor | 1050 ~ 1100 | 1000 ~ 1050 | 850 ~ 900 | Slow cooling (pit or sand cooling) |
Note: Cr12MoV steel has a low melting point, so the heating temperature should not be too high; it has poor thermal conductivity, so attention should be paid to slow heating. After forging, it must be cooled slowly to avoid cracks. It can be placed in a preheated pit and cooled to 400-500°C. Annealing can be performed after cooling.

Please fill out the following form to contact us now!
4. Heat Treatment of Cr12MoV Steel
4.1 Předehřívání
| Procesní parametry | |
|---|---|
| Post-Forging Annealing | Heating temperature 850 ~ 870°C, hold for 1 ~ 2h, furnace cool to below 500°C then air cool. Hardness after annealing is 207 ~ 255HBW, microstructure is fine pearlite + carbide. |
| Post-Forging Isothermal Annealing | Heating temperature 850 ~ 870°C, hold for 1 ~ 2h, furnace cool to 720 ~ 750°C, hold for 3 ~ 4h, furnace cool to below 550°C then air cool. Hardness after annealing is 207 ~ 255HBW. Microstructure is fine pearlite + carbide. |
| High-Temperature Tempering | Heating temperature 760 ~ 790°C, hold for 2 ~ 3h, furnace cool or air cool. Hardness is 207 ~ 255HBW. |
4.2 Kalení
Quenching Process Specifications for Cr12MoV Steel
| Systém | 1st Preheating Temp./°C | 2nd Preheating Temp./°C | Quenching Temp./°C | Kalící médium | Quenching Medium Temp./°C | Cooling in Medium | Subsequently | Tvrdost HRC |
| já | 550 ~ 600 | 840 ~ 860 | 950 ~ 1000 | Olej | 20 ~ 60 | To oil temp | Chlazení vzduchem | 58 ~ 62 |
| II | 1020 ~ 1040 | Olej | 20 ~ 60 | To oil temp | Chlazení vzduchem | 62 ~ 63 | ||
| III | 1020 ~ 1040 | Molten nitrate salt | 400 ~ 550 | 5 ~ 10min | Chlazení vzduchem | 62 ~ 63 | ||
| IV | 1115 ~ 1130 | Olej | 20 ~ 60 | To oil temp | Chlazení vzduchem | 42 ~ 50 | ||
| PROTI | 1115 ~ 1130 | Molten nitrate salt | 400 ~ 450 | 5 ~ 10min | Chlazení vzduchem | 42 ~ 50 |
Note: Schemes IV and V are used for molds that require hot hardness and high wear resistance, such as hot stamping dies working below 450°C, but their mechanical properties are poor, and dimensional deformation is large. After quenching according to schemes I and II, the volume fraction of the microstructure is 12% carbides, 68% to 73% martensite, and 20% to 25% retained austenit.
Hardness and Quenching Temperature Under Different Heating and Cooling Conditions
| Heating Conditions | Způsob chlazení | Quenching Temp./°C | Tvrdost HRC |
| Heating in carburizing agent | Oil cooling | 930 | 64 |
| 980 | 65 | ||
| 1010 | 65 | ||
| 1030 | 63.5 | ||
| Heating in air furnace | Oil cooling | 930 | 60.2 |
| 980 | 63 | ||
| 1010 | 63.9 | ||
| 1030 | 63.5 | ||
| Heating in air furnace | Chlazení vzduchem | 930 | 59 |
| 980 | 62.5 | ||
| 1010 | 63.2 | ||
| 1030 | 62 |
4.3 Temperování
Tempering Process Specifications
| Systém | Quenching Temp./°C | Účel temperování | Tempering Temp./°C | Střední | Tvrdost HRC |
| já | 1020 ~ 1040 | Stress relief | 150 ~ 170 | Oil or nitrate salt | 61 ~ 63 |
| II | Stress relief, reduce hardness | 200 ~ 275 | — | 57 ~ 59 | |
| III | 400 ~ 425 | — | 55 ~ 57 | ||
| IV | 1115 ~ 1130 | Stress relief and secondary hardening | 510 ~ 520℃ Multiple tempering | — | 60 ~ 61 |
| PROTI | -78℃ Cryogenic treatment + 510 ~ 520℃ single tempering | — | 60 ~ 61 | ||
| VI | -78℃ Cryogenic treatment plus one 510 ~ 520℃ tempering, then another -78℃ cryogenic treatment | — | 61 ~ 62 |
Poznámka:
- Workpieces tempered according to Scheme I need to maintain high hardness and high wear resistance, and their dimensional changes are almost independent of the quenching state.
- Scheme II is used to obtain workpieces with good toughness.
Tempering Temperature and Hardness
| Tempering Temp./°C | Netemperovaný | 100 | 200 | 300 | 400 | 500 | 550 | 600 | 650 |
|---|---|---|---|---|---|---|---|---|---|
| Tvrdost HRC | 63 | 62 | 61 | 59 | 57 | 59 | 53 | 47 | 40 |
Poznámka: Oil quenched at 1030°C, tempered for two hours.
5. Aplikace
Cr12MoV steel is suitable for manufacturing a wide variety of tools and dies that are characterized by large cross-sections, complex shapes, and are subjected to significant impact loads. Examples of such applications include:
- Punching dies with complex geometries
- General stamping dies
- Blanking dies for silicon steel sheets
- Ořezávání zemře
- Edge rolling/curling dies
- Tažírna drátu
- Vytlačování za studena umírá
- Deep drawing dies for steel plate
- Desky na válcování závitů
- Cold shearing blades
- Circular saws
- Standardní nástroje a měřidla
Prozkoumejte naše další produkty
D2/1.2379/SKD11
D3/1.2080/SKD1
D6/1,2436/SKD2
A2/1.23663/SKD12
O1/1.2510/SKS3
O2/1,2842
S1/1,2550
S7/1,2355
DC53
H13/1.2344/SKD61
H11/1.2343/SKD6
H21/1,2581/SKD7
L6/1.2714/SKT4
M2/1.3343/SKH51
M35/1.3243/SKH55
M42/1.3247/SKH59